A method for preparing co-extruded film for packaging

Through the seven-layer structure coextruded film preparation method and roller adjustment strategy, the problems of wrinkles and dislocations in coextruded film production are solved, product quality and production efficiency are improved, and excellent mechanical properties and ultraviolet protection properties are achieved.

CN118596617BActive Publication Date: 2024-11-22YANTAI EURASIA PLASTIC PACKAGING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410850311.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-22
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

In the production of coextruded film, wrinkles and roller misalignment of the surface of the coextruded film due to equipment, environment and operation problems, affecting the quality of cutting and winding products. Existing solutions such as replacing props and fine-tuning feeding devices cannot be effectively solved. These questions.

Method used

The coextruded film preparation method adopts a seven-layer structure, including a nylon layer, a blending layer, a barrier layer, an adhesive layer and a heat sealing layer. The relative position of the coextruded film and the roller are adjusted through the roller adjustment strategy, and the threshold value is determined and Distance calculation optimizes the roller movement strategy to ensure the stable conveying state of the coextruded film during cutting and winding.

Benefits of technology

The mechanical properties and UV resistance of the coextruded film are improved, the number of times of roller adjustment strategies is reduced, the production efficiency is improved, the friction is reduced, and the damage of pulling inaccuracy and excessive pulling force is ensured, ensuring product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118596617B_ABST
    Figure CN118596617B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of co-extruded film preparation, and discloses a method for preparing a co-extruded film for packaging, which is characterized by comprising: raw material pretreatment, melt extrusion, stretching cooling, cutting and winding; raw material pretreatment, respectively preparing the raw materials of the co-extruded film in proportion and then putting them into a mixer for uniform mixing, and then respectively sending them into an extruder for melting; melt extrusion, using an extruder to co-extrude and blow film to obtain a high-barrier co-extruded film; stretching cooling, applying tension and a coolant to the co-extruded film to stretch and cool the co-extruded film, and adopting a roller adjustment strategy. The method for preparing the co-extruded film for packaging determines whether the co-extruded film and the roller are misaligned by setting a range determined by a judgment threshold k. When the degree of offset between the co-extruded film and the roller is within the range determined by k, the impact on the subsequent cutting process is small, the number of times the roller adjustment strategy is adopted is reduced, and the efficiency of the co-extruded film production is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of co-extrusion film preparation, in particular to a method for preparing a co-extrusion film for packaging. Background Art

[0002] Co-extruded film is a special plastic packaging material. It combines the unique properties of each layer of material by simultaneously melting and blending multiple polymers during the extrusion process to form a single multi-layer structure. The structure of co-extruded film consists of multiple layers of polymers with different properties, which are tightly combined together through co-extrusion technology.

[0003] In actual production, equipment problems, environmental problems and operational problems cause wrinkles on the surface of the co-extruded film, and the co-extruded film and the roller are misaligned. After accumulation, the co-extruded film has unqualified product quality when cutting and winding. The existing solution is to replace the props and fine-tune the feeding device, but it does not solve the problem that the conveying state of the co-extruded film does not meet the cutting requirements after the co-extruded film and the roller are misaligned and wrinkled. Therefore, before cutting and winding, a set of roller adjustment strategies is required to adjust the position of the two ends of the roller, pull the co-extruded film from different directions and at different distances, solve the problem of wrinkles and misalignment of the co-extruded film, and prepare for the cutting and winding process. Summary of the invention

[0004] The present invention provides a method for preparing a co-extruded film for packaging, which helps solve the problem mentioned in the background technology that in actual production, due to equipment problems, environmental problems and operation problems, the surface wrinkles of the co-extruded film and the misalignment between the co-extruded film and the roller are caused, which accumulate and cause the product quality of the co-extruded film to be unqualified when cutting and winding. The existing solution is to replace the props and fine-tune the feeding device, but it does not solve the problem that after the co-extruded film and the roller are misaligned and wrinkled, the conveying state of the co-extruded film does not meet the cutting requirements.

[0005] The present invention provides the following technical solution: a method for preparing a co-extruded film for packaging, comprising:

[0006] Co-extruded film is divided into seven layers from inside to outside.

[0007] The first layer is a nylon layer, which is made of nylon material with a melting temperature of 230 degrees Celsius and a density of 1.13g / cm3;

[0008] The second layer is the first blended layer, which is composed of four raw materials: 30% metallocene polyethylene, 15% linear low-density polyethylene, 20% high-pressure polyethylene, and 35% polyolefin plastomer;

[0009] The third layer is the second blended layer, which is composed of two raw materials: 20% high-density polyethylene and 80% metallocene polyethylene;

[0010] The fourth layer is a barrier layer, which is composed of ethylene-vinyl alcohol copolymer resin;

[0011] The fifth layer is an adhesive layer, which is composed of a modified adhesive resin;

[0012] The sixth layer is the third blended layer, which is composed of four raw materials: 50% linear low-density polyethylene, 25% metallocene linear low-density polyethylene, 20% high-density polyethylene, and 5% black polyethylene masterbatch;

[0013] The seventh layer is a heat-sealing layer, which is composed of three raw materials: 20% low-density polyethylene, 78% metallocene polyethylene, and 2% Japanese Mitsui brand EZA-10 anti-blocking agent masterbatch.

[0014] As an optional scheme for the preparation method of the co-extruded film for packaging of the present invention, wherein: the total thickness of the co-extruded film is 45 μm-300 μm, and the thickness ratio of the first to seventh layers is 2:6:3:4:3:6:9.

[0015] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, the co-extruded film production step comprises:

[0016] The production process of co-extrusion film includes raw material pretreatment, melt extrusion, stretching cooling, cutting and winding.

[0017] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, the co-extruded film production step comprises:

[0018] Raw material pretreatment: the raw materials of the first to seventh layers of the co-extruded film are respectively prepared in proportion and put into a mixer for uniform mixing, and then respectively sent into an extruder for melting;

[0019] Melt extrusion, and a high barrier coextrusion film is coextruded and blown by an extruder according to the arrangement order of the first layer to the seventh layer;

[0020] Stretch cooling: apply tension and coolant to the coextruded film to stretch and cool the coextruded film. When the coextruded film and the roller move relative to each other, the roller adjustment strategy is adopted to adjust the relative position of the coextruded film and the roller.

[0021] Cutting refers to cutting the coextruded film by blade or thermal cutting;

[0022] Rewinding: Wind the cut co-extruded film onto a roll.

[0023] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, the roller adjustment strategy includes:

[0024] The two sides of the co-extruded film width are respectively the first side and the second side, the end of the roller close to the first side of the co-extruded film is the first end, the distance from the first end to the first side is recorded as w, the end of the roller close to the second side of the co-extruded film is the second end, and the distance from the second end to the second side is recorded as r;

[0025] The state in which the co-extruded film is stably conveyed on the roller is defined as the target state. When in the target state, the distance P from the first side of the co-extruded film to the first end = the distance Q from the second side of the co-extruded film to the second end = (the width of the roller - the width of the co-extruded film) ÷ 2;

[0026] The number of rollers used in the roller adjustment strategy is counted, recorded as n, and the first roller that the co-extruded film passes through after cooling and stretching is recorded as the first roller, the second roller that passes through is recorded as the second roller... The nth roller that passes through is called the nth roller, and the n rollers are arranged horizontally in parallel;

[0027] The judgment threshold of the co-extruded film misalignment is k. When |rQ|>Q*k or |wP|>P*k, the roller adjustment strategy is adopted to adjust the position of the co-extruded film and the roller.

[0028] The judgment threshold k is used to judge the degree of lateral deviation between the co-extruded film and the roller. When the lateral deviation of the co-extruded film exceeds the range determined by k, the co-extruded film is misaligned. When |rQ|≦Q*k and |wP|≦P*k, the co-extruded film is in a stable conveying state.

[0029] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, wherein: the position of the co-extruded film is adaptively adjusted by adjusting the first end and the second end of the roller, wherein the universal distance u and the special distance v are set to characterize the required moving distance of the first end or the second end of the roller;

[0030] When w>P*(1+k) and r>Q*(1+k), let Δw=wP, Δr=rQ

[0031] but:

[0032] When the co-extruded film passes through each roller from the first roller to the nth roller, the distance between the first end and the second end of the roller is reduced by v+u, the first side of the co-extruded film is pulled toward the first end of the roller by a distance Δw÷n, and the second side of the co-extruded film is pulled toward the second end of the roller by a distance Δr÷n.

[0033] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, wherein:

[0034] When w=P and r>Q*(1+k), let Δr=rQ.

[0035] but:

[0036] When the coextruded film passes through each of the rollers from the first roller to the nth roller, reduce the distance v + u at the second end of the roller, increase the distance u at the first end of the roller, and pull the second side of the coextruded film to move a distance of Δr÷n in the direction of the second end of the roller;

[0037] When r = Q and w > P*(1 + k), record Δw = w - P,

[0038] Then:

[0039] When the coextruded film passes through each of the rollers from the first roller to the nth roller, reduce the distance v + u at the first end of the roller, increase the distance u at the second end of the roller, and pull the first side of the coextruded film to move a distance of Δw÷n in the direction of the first end of the roller.

[0040] As an alternative embodiment of the method for preparing the coextruded film for packaging according to the present invention, wherein:

[0041] When w < P*(1 - k) and r > Q*(1 + k), record Δw = P - w, Δr = r - Q,

[0042] If the coextruded film does not wrinkle,

[0043] Then:

[0044] When the coextruded film passes through each of the rollers from the first roller to the nth roller, reduce the distance u at the first end and the second end of the roller, and pull the second side of the coextruded film to move a distance of Δr÷n in the direction of the second end of the roller;

[0045] If the coextruded film wrinkles,

[0046] When the coextruded film passes through each of the rollers from the first roller to the (n - 1)th roller, reduce the distance v + u at the first end and the second end of the roller, and pull the second side of the coextruded film to move a distance of Δr÷(n - 1) in the direction of the second end of the roller,

[0047] When the coextruded film passes through the nth roller, raise the second end of the roller by 2*u + v, and pull the first side of the coextruded film to the position of the stable conveying state of the coextruded film;

[0048] When r < Q*(1 - k) and w > P*(1 + k), record Δr = Q - r, Δw = w - P,

[0049] If the coextruded film does not wrinkle,

[0050] Then:

[0051] When the coextruded film passes through each of the rollers from the first roller to the nth roller, reduce the distance u at the first end and the second end of the roller, and pull the first side of the coextruded film to move a distance of Δw÷n in the direction of the first end of the roller;

[0052] If the coextruded film wrinkles,

[0053] When the co-extruded film passes through each roller from the first roller to the n-1 roller, the distance between the first end and the second end of the roller is reduced by a distance v+u, and the first side of the co-extruded film is pulled toward the first end of the roller to move a distance Δw÷(n-1).

[0054] When the co-extruded film passes through the nth roller, the first end of the roller is raised by a distance of 2*u+v, and the second side of the co-extruded film is pulled toward the second end of the roller to a position where the co-extruded film is stably conveyed.

[0055] As an optional solution of the method for preparing the co-extruded film for packaging of the present invention, the setting of the universal distance u and the special distance v to characterize the required moving distance of the first end or the second end of the roller includes:

[0056] The maximum distance from the protruding point of the co-extruded film to the roller is measured, recorded as s, and the threshold for judging the wrinkles of the co-extruded film is given as h.

[0057] If s>h, the coextruded film is wrinkled, and the roller adjustment strategy is adopted for the coextruded film;

[0058] The distances from all points on the folds of the co-extruded film using the roller adjustment strategy to the roller are counted, and the mean of the above distances is calculated as the special distance v;

[0059] The roller is removed and the flat co-extruded film is measured. When the co-extruded film loses the support force of the roller and becomes concave, the maximum depth of the concave co-extruded film is the universal distance u.

[0060] The present invention has the following beneficial effects:

[0061] The preparation method of the co-extruded film for packaging is that the second layer of the co-extruded film is compounded with raw materials of specific types and proportions, which can make the co-extruded film have excellent mechanical properties, especially ensure the mechanical properties of the co-extruded film in a low-temperature environment, thereby reducing the package breakage rate of the co-extruded film in a low-temperature environment; the sixth layer is made by different raw material selections, adding an anti-ultraviolet agent, and mixing a black masterbatch into the interlayer co-extrusion to achieve the anti-ultraviolet and high light-shielding properties of the co-extruded film.

[0062] 2. The preparation method of the co-extruded film for packaging determines whether the co-extruded film and the roller are misaligned by setting a range determined by a judgment threshold k. When the degree of misalignment between the co-extruded film and the roller is within the range determined by k, the impact on the subsequent cutting process is small, the number of times the roller adjustment strategy is adopted is reduced, and the efficiency of the co-extruded film production is improved.

[0063] 3. The preparation method of the co-extruded film for packaging, by calculating the general distance u, when the co-extruded film does not wrinkle, the distance u between the first end and the second end of the roller is reduced, the co-extruded film and the roller do not contact, and the friction between the roller and the co-extruded film is prevented, which affects the accuracy of pulling the co-extruded film. By calculating the special distance v, when the co-extruded film wrinkles and the roller adjustment strategy is required, the distance u+v between the first end and the second end of the roller is reduced, the co-extruded film and the roller do not contact, and the friction between the roller and the co-extruded film is prevented, which affects the accuracy of pulling the co-extruded film. When the distance u of the first end or the second end of the roller is raised, the second end or the first end of the roller is lowered u+v, the co-extruded film at one end of the roller is not in contact with the roller, and the side of the co-extruded film contacting the roller can be pulled, and the co-extruded film at one end of the roller is raised to contact the roller, and the side of the co-extruded film contacting the roller remains unchanged in the position of the roller, so that the co-extruded film can be pulled from different directions and at different distances.

[0064] 4. In the preparation method of the co-extruded film for packaging, in the roller adjustment strategy, the total distance moved by the co-extruded film is calculated, the total distance is evenly divided on each roller, and the co-extruded film is pulled on each roller by the evenly divided distance to prevent the co-extruded film from being damaged due to excessive pulling force when the co-extruded film is pulled on one roller for too long.

[0065] 5. The preparation method of the co-extruded film for packaging is characterized in that a threshold value h for judging the wrinkles of the co-extruded film is given. When the unevenness of the co-extruded film exceeds the threshold value, a roller adjustment strategy is adopted. When the unevenness of the co-extruded film does not exceed the threshold value, the subsequent cutting process of the co-extruded film is less affected. At the same time, the number of times the roller adjustment strategy is adopted is reduced, thereby improving the efficiency of the co-extruded film production. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 This is a schematic structural diagram of the co-extruded film and rollers in a state where the co-extruded film is stably conveyed according to the present invention.

[0067] Figure 2 This is a structural schematic diagram of a situation in which the co-extruded film of the present invention is wrinkled and both sides are misaligned.

[0068] Figure 3 This is a structural schematic diagram of a situation in which the co-extruded film of the present invention is wrinkled and one side is misaligned.

[0069] Figure 4 This is a second structural schematic diagram of a situation in which the co-extruded film of the present invention is wrinkled and one side is misaligned.

[0070] Figure 5 This is a schematic structural diagram of the second situation in which the co-extruded film of the present invention is wrinkled and both sides are misaligned.

[0071] Figure 6 Schematic diagram of the third structure of the co-extruded film of the present invention in which wrinkles occur and both sides are misaligned.

[0072] Figure 7 It is a structural schematic diagram of a situation where both sides of the co-extruded film of the present invention are misaligned when no wrinkles occur.

[0073] Figure 8 This is a second structural schematic diagram of the situation where both sides of the co-extruded film of the present invention are misaligned when no wrinkles occur.

[0074] Fig. 9 A schematic diagram of a situation in which a roller adjustment strategy is required when wrinkles occur in the co-extruded film of the present invention;

[0075] Fig.10 A schematic diagram of the structure of a high-barrier co-extruded film provided by the present invention;

[0076] Fig.11 A schematic diagram of the roller structure of the roller adjustment device provided by the present invention;

[0077] In the figure: 01, roller, 02, co-extruded film, 03, first side of the co-extruded film, 04, second side of the co-extruded film, 05, first end of the roller, 06, second end of the roller, 07, edge position of the first end of the roller, 08, position of the first side of the co-extruded film when it is stably conveyed, 09, position of the second side of the co-extruded film when it is stably conveyed, 10, edge position of the second end of the roller, 11, maximum distance from the raised point of the uneven part of the co-extruded film to the roller, A-nylon layer, B-first blended layer, C-second blended layer, D-barrier layer, E-adhesive layer, F-third blended layer, G-heat sealing layer. DETAILED DESCRIPTION

[0078] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0079] Example 1

[0080] Co-extruded film is divided into seven layers from inside to outside.

[0081] The first layer is a nylon layer, which is made of nylon material with a melting temperature of 230 degrees Celsius and a density of 1.13g / cm3;

[0082] The second layer is the first blended layer, which is composed of four raw materials: 30% metallocene polyethylene, 15% linear low-density polyethylene, 20% high-pressure polyethylene, and 35% polyolefin plastomer;

[0083] The third layer is the second blended layer, which is composed of two raw materials: 20% high-density polyethylene and 80% metallocene polyethylene;

[0084] The fourth layer is a barrier layer, which is composed of ethylene-vinyl alcohol copolymer resin;

[0085] The fifth layer is an adhesive layer, which is composed of a modified adhesive resin;

[0086] The sixth layer is the third blended layer, which is composed of four raw materials: 50% linear low-density polyethylene, 25% metallocene linear low-density polyethylene, 20% high-density polyethylene, and 5% black polyethylene masterbatch;

[0087] The seventh layer is a heat-sealing layer, which is composed of three raw materials: 20% low-density polyethylene, 78% metallocene polyethylene, and 2% Japanese Mitsui brand EZA-10 anti-blocking agent masterbatch.

[0088] The total thickness of the co-extruded film is 45 μm-300 μm, and the thickness ratio of the first layer to the seventh layer is 2:6:3:4:3:6:9.

[0089] The co-extrusion film production steps include:

[0090] The production process of co-extrusion film includes raw material pretreatment, melt extrusion, stretching cooling, cutting and winding.

[0091] Raw material pretreatment: the raw materials of the first to seventh layers of the co-extruded film are respectively prepared in proportion and put into a mixer for uniform mixing, and then respectively sent into an extruder for melting;

[0092] Melt extrusion, in the order of the first layer to the seventh layer, using an extruder to co-extrude and blow film to obtain a high-barrier co-extruded film;

[0093] Stretch cooling: apply tension and coolant to the coextruded film to stretch and cool the coextruded film. When the coextruded film and the roller move relative to each other, the roller adjustment strategy is adopted to adjust the relative position of the coextruded film and the roller.

[0094] Cutting refers to cutting the coextruded film by blade or thermal cutting;

[0095] Rewinding: Wind the cut co-extruded film onto a roll.

[0096] The roller adjustment strategy includes:

[0097] The two sides of the co-extruded film width are respectively the first side and the second side, the end of the roller close to the first side of the co-extruded film is the first end, the distance from the first end to the first side is recorded as w, the end of the roller close to the second side of the co-extruded film is the second end, and the distance from the second end to the second side is recorded as r;

[0098] The state in which the co-extruded film is stably conveyed on the roller is defined as the target state. When in the target state, the distance P from the first side of the co-extruded film to the first end = the distance Q from the second side of the co-extruded film to the second end = (the width of the roller - the width of the co-extruded film) / 2;

[0099] like Figure 1 As shown, in this example, the width of the co-extruded film is measured to be 10 dm, the length of the roller is measured to be 18 dm, and when the co-extruded film is in a stable conveying state on the roller, the distance P from the first side of the co-extruded film to the first end = the distance Q from the second side of the co-extruded film to the second end = (18-10) / 2 = 4 dm;

[0100] The number of rollers used in the roller adjustment strategy is counted and recorded as n. The first roller that the co-extruded film passes through after cooling and stretching is called the first roller, the second roller it passes through is called the second roller... The nth roller it passes through is called the nth roller, and the n rollers are arranged horizontally in parallel.

[0101] like Fig.11 As shown, in this example, the number of rollers of the roller adjustment device is 5, which are respectively called the first roller, the second roller, the third roller, the fourth roller and the fifth roller.

[0102] In the roller adjustment strategy, the total distance that the co-extruded film moves is calculated, and the total distance is evenly divided on each roller. The co-extruded film is pulled on each roller by the evenly divided distance to prevent the co-extruded film from being damaged due to excessive pulling force when the co-extruded film is pulled on one roller for too long.

[0103] The judgment threshold of the co-extruded film misalignment is k. When |rQ|>Q*k or |wP|>P*k, the roller adjustment strategy is adopted to adjust the position of the co-extruded film and the roller.

[0104] The judgment threshold k is used to judge the degree of lateral deviation between the co-extruded film and the roller. When the co-extruded film deviates beyond the range determined by k, the co-extruded film is misaligned. When |rQ|≦Q*k and |wP|≦P*k, the co-extruded film is in a stable conveying state.

[0105] By setting the range determined by the judgment threshold k, it is determined whether the co-extruded film and the roller are misaligned. When the degree of displacement between the co-extruded film and the roller is within the range determined by k, the impact on the subsequent cutting process is small, which reduces the number of times the roller adjustment strategy is adopted and improves the efficiency of co-extruded film production. Generally speaking, the co-extruded film cutting process requires the relative position deviation of the co-extruded film and the roller to be within 5%. Therefore, the value of k used to determine the degree of lateral displacement between the co-extruded film and the roller is 5%.

[0106] The method of adaptively adjusting the position of the co-extruded film by adjusting the first end and the second end of the roller, wherein the universal distance u and the special distance v are set to characterize the required moving distance of the first end or the second end of the roller; comprises:

[0107] The maximum distance from the protruding point of the co-extruded film to the roller is measured, recorded as s, and the threshold for judging the wrinkles of the co-extruded film is given as h.

[0108] If s>h, the coextruded film is wrinkled, and the roller adjustment strategy is adopted for the coextruded film;

[0109] like Fig. 9 As shown, in this example, the threshold value h=0.1dm. When wrinkles occur in the co-extruded film, the maximum value s of the distance from the raised point at the wrinkle to the roller is 0.15, which exceeds the threshold value h. The co-extruded film needs to adopt a roller adjustment strategy.

[0110] The distances from all points on the wrinkles of the co-extruded film using the roller adjustment strategy to the roller are counted, and the average of the above distances is calculated to be the special distance v. When the co-extruded film is wrinkled, the roller is removed and the co-extruded film is deformed. The deformed part of the co-extruded film is the part of the co-extruded film that was originally raised by the support force of the roller. After the roller is removed, it sags downward, and the average distance of the downward depression is approximately equal to the special distance v. Therefore, in order to ensure that the co-extruded film and the roller are not in contact, the roller needs to be moved a distance of v+u.

[0111] Remove the roller and measure the flat co-extruded film. When the co-extruded film loses the support of the roller and sinks, the maximum depth of the co-extruded film is the universal distance u.

[0112] By calculating the universal distance u, when the co-extruded film is not wrinkled, the distance u between the first end and the second end of the roller is reduced, and the co-extruded film and the roller are not in contact, thereby preventing the roller and the co-extruded film from contacting and generating friction, which affects the accuracy of pulling the co-extruded film. Taking the example of the present invention as an example, the universal distance u of the co-extruded film is measured to be 0.2dm.

[0113] By calculating the special distance v, when the co-extruded film is wrinkled, the distance u+v between the first end and the second end of the roller is reduced, and the co-extruded film and the roller are not in contact, which prevents the friction generated by the contact between the roller and the co-extruded film and affects the accuracy of pulling the co-extruded film. In actual application, the special distance will change with the movement of the co-extruded film.

[0114] When the first end or the second end of the roller is raised by a distance u, and the second end or the first end of the roller is lowered by a distance u+v, the coextruded film at one end of the lowered roller does not contact the roller, and the side of the coextruded film contacting the roller can be pulled. When the coextruded film at one end of the raised roller contacts the roller, the side of the coextruded film contacting the roller remains unchanged on the roller, and the coextruded film can be pulled from different directions and at different distances.

[0115] In this example, the wrinkles of the co-extruded film all represent that the maximum distance s from the protruding point of the uneven part of the co-extruded film to the roller is greater than the threshold value h, and a roller adjustment strategy needs to be adopted.

[0116] When w>P*(1+k) and r>Q*(1+k), let Δw=wP, Δr=rQ

[0117] but:

[0118] When the co-extruded film passes through each roller from the first roller to the nth roller, the distance between the first end and the second end of the roller is reduced by v+u, the first side of the co-extruded film is pulled toward the first end of the roller by a distance Δw÷n, and the second side of the co-extruded film is pulled toward the second end of the roller by a distance Δr÷n.

[0119] like Figure 2 As shown, in this example, w=4.3dm, r=4.5dm, that is, when w>P*(1+k) and r>Q*(1+k), Δw=wP=0.3dm, Δr=rQ=0.5dm,

[0120] The maximum distance from the uneven point of the co-extruded film to the roller is s=0.12, s>h, the co-extruded film is wrinkled, and the special distance v=0.2dm is measured.

[0121] When the co-extruded film passes through each roller from the first roller to the fifth roller, the distance between the first end and the second end of the roller is lowered by 0.4dm, the co-extruded film and the roller are not in contact, the first side edge of the co-extruded film is pulled toward the first end of the roller by 0.06dm, and the second side edge of the co-extruded film is pulled toward the second end of the roller by 0.1dm.

[0122] When w=P and r>Q*(1+k), let Δr=rQ.

[0123] but:

[0124] When the co-extruded film passes through each roller from the first roller to the nth roller, the second end of the roller is lowered by a distance v+u, the first end of the roller is raised by a distance u, and the second side of the co-extruded film is pulled toward the second end of the roller to move a distance Δr÷n;

[0125] like Figure 3 As shown, in this example, w=4dm, r=4.4dm, that is, when w=P and r>Q*(1+k), Δr=rQ=0.4dm,

[0126] The maximum distance from the protruding point of the co-extruded film to the roller is s=0.14, s>h, and the co-extruded film is wrinkled. The special distance v=0.11dm is measured at this time.

[0127] When the co-extruded film passes through each roller from the first roller to the fifth roller, lower the second end of the roller by a distance of 0.31 dm and raise the first end of the roller by a distance of 0.2 dm. The first side of the co-extruded film contacts the roller, and the position of the first side on the roller remains unchanged. The second side does not contact the roller, and pull the second side of the co-extruded film in the direction of the second end of the roller to move a distance of 0.08 dm.

[0128] When r = Q and w > P*(1 + k), let Δw = w - P.

[0129] Then:

[0130] When the co-extruded film passes through each roller from the first roller to the nth roller, lower the first end of the roller by a distance of v + u and raise the second end of the roller by a distance of u, and pull the first side of the co-extruded film in the direction of the first end of the roller to move a distance of Δw÷n.

[0131] As Figure 4 shown, in this example, it is measured that w = 5.0 dm, r = 4 dm, that is, when r = Q and w > P*(1 + k), Δw = w - P = 1 dm.

[0132] It is measured that the maximum distance from the raised point of the unevenness of the co-extruded film to the roller is s = 0.18, s > h, and the co-extruded film wrinkles. It is measured that the special distance v of the co-extruded film is 0.25 dm.

[0133] When the co-extruded film passes through each roller from the first roller to the fifth roller, lower the first end of the roller by 0.45 dm and raise the second end of the roller by a distance of 0.2 dm. The second side of the co-extruded film contacts the roller, and the position of the second side on the roller remains unchanged. The first side does not contact the roller, and pull the first side of the co-extruded film in the direction of the first end of the roller to move a distance of 0.2 dm.

[0134] When w < P*(1 - k) and r > Q*(1 + k), let Δw = P - w, Δr = r - Q.

[0135] If the co-extruded film does not wrinkle,

[0136] Then:

[0137] When the co-extruded film passes through each roller from the first roller to the nth roller, lower the first end and the second end of the roller by a distance of u, and pull the second side of the co-extruded film in the direction of the second end of the roller to move a distance of Δr÷n.

[0138] As Figure 7 shown, in this example, it is measured that w = 3.5 dm, r = 4.5 dm, that is, when w < P*(1 - k) and r > Q*(1 + k), Δw = P - w = 0.5 dm, Δr = r - Q = 0.5 dm.

[0139] The maximum distance s from the raised point of the uneven co-extruded film to the roller is measured as s = 0, s < h, and the co-extruded film does not wrinkle.

[0140] When the co-extruded film passes through each roller from the first roller to the fifth roller, lower the distance between the first end and the second end of the roller by 0.2 dm. The co-extruded film does not contact the roller, and pull the second side of the co-extruded film 0.1 dm in the direction of the second end of the roller.

[0141] If the co-extruded film develops wrinkles,

[0142] When the co-extruded film passes through each roller from the first roller to the (n - 1)-th roller, lower the distance between the first end and the second end of the roller by v + u, and pull the second side of the co-extruded film Δr÷(n - 1) in the direction of the second end of the roller.

[0143] When the co-extruded film passes through the n-th roller, raise the second end of the roller by 2*u + v, and pull the first side of the co-extruded film to the position of the stable conveying state of the co-extruded film in the direction of the first end of the roller.

[0144] As Figure 5 shown, in this example, it is measured that w = 3.5 dm, r = 5 dm, that is, w < P*(1 - k) and r > Q*(1 + k), Δw = P - w = 0.5 dm, Δr = r - Q = 1 dm.

[0145] The maximum distance s from the raised point of the uneven co-extruded film to the roller is measured as s = 0.14, s > h, the co-extruded film wrinkles, and the special distance v of the co-extruded film is measured as 0.12 dm.

[0146] When the co-extruded film passes through each roller from the first roller to the fourth roller, lower the distance between the first end and the second end of the roller by 0.32 dm. The co-extruded film does not contact the roller, and pull the second side of the co-extruded film 0.25 dm in the direction of the second end of the roller.

[0147] When the co-extruded film passes through the fifth roller, raise the second end of the roller by 0.52 dm. The second side of the co-extruded film contacts the roller, and the position of the second side on the roller remains unchanged. The first side does not contact the roller, and pull the first side of the co-extruded film to the position of the stable conveying state of the co-extruded film in the direction of the first end of the roller.

[0148] When r < Q*(1 - k) and w > P*(1 + k), denote Δr = Q - r, Δw = w - P.

[0149] If the co-extruded film does not wrinkle,

[0150] Then:

[0151] When the coextruded film passes through each of the rollers from the first roller to the nth roller, reduce the distance u between the first end and the second end of the roller, and pull the first side of the coextruded film in the direction of the first end of the roller to move a distance of Δw÷n.

[0152] As Figure 8 shown, in this example, it is measured that w = 4.5 dm and r = 3.5 dm, that is, r < Q*(1 - k) and w > P*(1 + k). Denote Δw = w - P = 0.5 dm and Δr = Q - r = 0.5 dm.

[0153] The maximum distance from the raised point of the unevenness of the coextruded film to the roller is measured and denoted as s = 0, s < h, and the coextruded film does not wrinkle.

[0154] When the coextruded film passes through each of the rollers from the first roller to the 5th roller, reduce the distance between the first end and the second end of the roller by 0.2 dm. The coextruded film does not contact the roller, and pull the first side of the coextruded film in the direction of the first end of the roller to move a distance of 0.1 dm.

[0155] If the coextruded film sends wrinkles,

[0156] When the coextruded film passes through each of the rollers from the first roller to the (n - 1)th roller, reduce the distance v + u between the first end and the second end of the roller, and pull the first side of the coextruded film in the direction of the first end of the roller to move a distance of Δw÷(n - 1).

[0157] When the coextruded film passes through the nth roller, raise the first end of the roller by a distance of 2*u + v, and pull the second side of the coextruded film in the direction of the second end of the roller to the position of the stable conveying state of the coextruded film.

[0158] As Figure 6 shown, in this example, it is measured that w = 5 dm and r = 3.5 dm, that is, w > P*(1 + k) and r < Q*(1 - k), Δw = w - P = 1 dm, and Δr = Q - r = 0.5 dm.

[0159] The maximum distance s from the raised point of the unevenness of the coextruded film to the roller is measured as s = 0.14, s > h, the coextruded film wrinkles, and the special distance v of the coextruded film is measured as 0.12 dm.

[0160] When the coextruded film passes through each of the rollers from the first roller to the 4th roller, reduce the distance between the first end and the second end of the roller by 0.32 dm. The coextruded film does not contact the roller, and pull the first side of the coextruded film in the direction of the first end of the roller to move a distance of 0.2 dm.

[0161] When the co-extruded film passes through the 5th roller, the first end of the roller is raised by 0.52dm, the first side of the co-extruded film contacts the roller, the position of the first side on the roller remains unchanged, the second side does not contact the roller, and the second side of the co-extruded film is pulled toward the second end of the roller to a position where the co-extruded film is in a stable conveying state.

[0162] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0163] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a co-extruded film for packaging, characterized in that: include: Raw material pretreatment, melt extrusion, stretching cooling, cutting and winding; Raw material pretreatment: the raw materials for the co-extrusion film are mixed in proportion and then put into a mixer for uniform mixing, and then sent to the extruder for melting; Melt extrusion, using an extruder to co-extrude and blow film to produce a high-barrier co-extruded film; Stretch cooling: applying tension and coolant to the coextruded film to stretch and cool the coextruded film. When the coextruded film and the roller move relative to each other, the roller adjustment strategy is adopted to adjust the relative position of the coextruded film and the roller. The roller adjustment strategy is specifically as follows: The two sides of the co-extruded film width are respectively the first side and the second side, the end of the roller close to the first side of the co-extruded film is the first end, and the distance from the first end to the first side is w. The end of the roller close to the second side of the co-extruded film is the second end, and the distance from the second end to the second side is r; Define the state of the co-extruded film being stably conveyed on the roller as the target state. When in the target state, the distance P from the first side of the co-extruded film to the first end = the distance Q from the second side of the co-extruded film to the second end = (the width of the roller - the width of the co-extruded film) ÷ 2; The number of rollers used in the roller adjustment strategy is counted, recorded as n, the first roller that the co-extruded film passes through after cooling and stretching is the first roller, the second roller that the co-extruded film passes through is the second roller, and the nth roller that the co-extruded film passes through is called the nth roller. The n rollers are arranged horizontally in parallel. The threshold value of the co-extruded film misalignment is k. When |rQ|>Q*k or |wP|>P*k, Then, the roller adjustment strategy is adopted to adjust the positions of the co-extruded film and the roller; The determination threshold k is used to determine the extent of lateral deviation between the co-extruded film and the roller. When the lateral deviation of the co-extruded film exceeds the range determined by k, the co-extruded film is misaligned. When |rQ|≦Q*k and |wP|≦P*k, the co-extruded film is in a stable conveying state; Adaptively adjusting the position of the coextruded film by adjusting the first end and the second end of the roller, wherein the universal distance u and the special distance v are set to characterize the required moving distance of the first end or the second end of the roller; Among them, the setting method of general distance u and special distance v is as follows: The maximum distance from the protruding point of the co-extruded film to the roller is measured, recorded as s, and the threshold for judging the wrinkles of the co-extruded film is given as h. If s>h, the coextruded film is wrinkled, and the roller adjustment strategy is adopted for the coextruded film; The distances from all points on the folds of the co-extruded film using the roller adjustment strategy to the roller are counted, and the mean of the above distances is calculated as the special distance v; Remove the roller and measure the maximum depth of the flat co-extruded film when it loses the support of the roller and sinks, which is the universal distance u. When w>P*(1+k) and r>Q*(1+k), let Δw=wP, Δr=rQ but: When the coextruded film passes through each roller from the first roller to the nth roller, Lower the distance v+u between the first end and the second end of the roller, pull the first side of the co-extruded film toward the first end of the roller by a distance Δw÷n, and pull the second side of the co-extruded film toward the second end of the roller by a distance Δr÷n; When w=P and r>Q*(1+k), let Δr=rQ. but: When the coextruded film passes through each roller from the first roller to the nth roller, Reduce the distance v + u at the second end of the roller, increase the distance u at the first end of the roller, and pull the second side of the coextruded film towards the second end of the roller by a distance of Δr÷n; When r = Q and w > P*(1 + k), let Δw = w - P, Then: When the coextruded film passes through each roller from the first roller to the nth roller, reduce the distance v + u at the first end of the roller, increase the distance u at the second end of the roller, and pull the first side of the coextruded film towards the first end of the roller by a distance of Δw÷n; When w < P*(1 - k) and r > Q*(1 + k), let Δw = P - w, Δr = r - Q, If the coextruded film does not wrinkle, Then: When the coextruded film passes through each roller from the first roller to the nth roller, reduce the distance u at the first end and the second end of the roller, and pull the second side of the coextruded film towards the second end of the roller by a distance of Δr÷n; If the coextruded film wrinkles, When the coextruded film passes through each roller from the first roller to the (n - 1)th roller, reduce the distance v + u at the first end and the second end of the roller, and pull the second side of the coextruded film towards the second end of the roller by a distance of Δr÷(n - 1), When the coextruded film passes through the nth roller, increase the distance 2*u + v at the second end of the roller, and pull the first side of the coextruded film towards the first end to the position of the stable conveying state of the coextruded film; When r < Q*(1 - k) and w > P*(1 + k), let Δr = Q - r, Δw = w - P, If the coextruded film does not wrinkle, Then: When the coextruded film passes through each roller from the first roller to the nth roller, reduce the distance u at the first end and the second end of the roller, and pull the first side of the coextruded film towards the first end by a distance of Δw÷n; If the coextruded film wrinkles, When the coextruded film passes through each roller from the first roller to the (n - 1)th roller, reduce the distance v + u at the first end and the second end of the roller, and pull the first side of the coextruded film towards the first end by a distance of Δw÷(n - 1), When the coextruded film passes through the nth roller, increase the distance 2*u + v at the first end of the roller, and pull the second side of the coextruded film towards the second end to the position of the stable conveying state of the coextruded film; Cutting, cutting the coextruded film by means of a blade or thermal cutting; Rewinding, winding the cut coextruded film onto a reel for rewinding.

Citation Information

Patent Citations

  • All-plastic gas phase rust prevention complex film and production method thereof

    CN101579956A

  • Method for longitudinal stretching a film in solid state and apparatus to carry out the method

    CN102414010A

  • Fusion cutting guide device and method suitable for film bodies with different thicknesses of plastic packaging bags

    CN115107320A

  • Method for producing stretched film

    CN115139505A

  • Pressing mechanism for film material winding device and film material winding device applying pressing mechanism