A bio-based polyurethane material and its preparation method and application

By preparing flame-retardant ammonia pellets and reacting enzymatic lignin with isocyanate, the problem of insufficient mechanical properties and flame retardancy of bio-based polyurethane materials is solved, and cost reduction and performance improvement are achieved. It is suitable for water-based polyurethane coatings.

CN118652410BActive Publication Date: 2024-11-29GUANGZHU COLORTECH NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411139594.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing bio-based polyurethane materials have shortcomings in terms of mechanical properties and flame retardancy, and the production costs are high, making it difficult to meet industrial needs.

Method used

Flame-retardant ammonia pellets were prepared by reacting modified nanosilane coupling agent with phosphorus oxychloride, and the bio-based polyurethane was prepared by extracting and enzymatic lignin with deep eutectic solvents, and bio-based polyurethane was prepared by reacting with isocyanate. Material.

Benefits of technology

It improves the mechanical properties and flame retardant properties of bio-based polyurethane materials, reduces production costs, and enhances the degradability of the materials. It is suitable for water-based polyurethane coatings and meets industrial needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention proposes a bio-based polyurethane material and a preparation method and application thereof, belonging to the technical field of polyurethane. Nano-silica microspheres are modified by aminosilane coupling agents and reacted with phosphorus oxychloride to obtain flame-retardant aminated beads; after straw lignin is extracted by deep eutectic solvent, enzymatic hydrolysis is obtained, and the enzymatic hydrolyzed lignin is reacted with isocyanate together with the flame-retardant aminated beads to obtain a bio-based polyurethane material. The bio-based polyurethane material prepared by the present invention uses agricultural byproduct straw as raw material, which greatly improves the degradability of the prepared material, reduces production costs, and improves the environmental friendliness of the material. At the same time, the prepared material has good mechanical properties and flame retardant properties, can meet industrial needs, can be used to prepare waterborne polyurethane coatings, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyurethane, and in particular to a bio-based polyurethane material and a preparation method and application thereof. Background Art

[0002] Polyurethane (PU) is usually composed of soft segment diol oligomers, hard segment isocyanate and chain extender. The performance difference between the soft segment and the hard segment leads to microphase separation. By adjusting the ratio of the soft and hard segments, the strength and toughness of polyurethane can be regulated. At present, polyurethane materials synthesized from non-renewable fossil raw materials have stable chemical properties and are widely used, but they are difficult to degrade in the natural environment after being discarded, causing serious environmental pollution. Therefore, effectively using renewable bio-based raw materials to replace petroleum-based raw materials to produce PU has become a research focus.

[0003] At present, the research on bio-based polyurethanes mainly focuses on isocyanate-free PU, biomass chain extender PU and bio-based polyol isocyanate PU. Among them, the production technology of isocyanate-free PU is still in the development stage and the cost is relatively high. Biomass chain extender PU can replace part of the petroleum-based chain extender and be used as the chain extension of PU, but its ability to increase the bio-based content of PU is limited.

[0004] At present, the application prospect of using bio-based polyols to replace petroleum-based polyols to produce bio-based PU is good. Most bio-based polyols come from vegetable oils or lignin and its derivatives. Vegetable oils, as a typical renewable biomass resource, have a simple structure and low price, and have great advantages in the development of biomass materials. However, PU made from biological sources often has problems such as poor mechanical properties and poor flame retardancy. Summary of the invention

[0005] The purpose of the present invention is to propose a bio-based polyurethane material and a preparation method and application thereof, which uses agricultural by-product straw as raw material, greatly improves the degradability of the prepared material, reduces production costs, and improves the environmental friendliness of the material. At the same time, the prepared material has good mechanical properties and flame retardant properties, can meet industrial needs, can be used to prepare water-based polyurethane coatings, and has broad application prospects.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The invention provides a method for preparing a bio-based polyurethane material. Nano-silica microspheres are modified by an aminosilane coupling agent and reacted with phosphorus oxychloride to obtain flame-retardant aminated small balls. Straw lignin is extracted by a deep eutectic solvent and then subjected to enzymolysis to obtain enzymolyzed lignin. The enzymolyzed lignin is reacted with isocyanate together with the flame-retardant aminated small balls to obtain a bio-based polyurethane material.

[0008] As a further improvement of the present invention, the following steps are included:

[0009] S1. Preparation of aminated beads: adding nano-silica microspheres to ethanol, adding a composite aminosilane coupling agent, heating and stirring the reaction, centrifuging, washing, and drying to obtain aminated beads;

[0010] S2. Preparation of flame retardant aminated pellets: The aminated pellets and phosphorus oxychloride were added to ethyl acetate, heated and stirred to react, centrifuged, washed, and dried to obtain flame retardant aminated pellets;

[0011] S3. Extraction of lignin: The straw is crushed, added to a deep eutectic solvent, heated and stirred for extraction, cooled, centrifuged, the liquid is precipitated with water, filtered, the solid is washed, and dried to obtain lignin;

[0012] S4. Enzymatic hydrolysis of lignin: adding lignin to water, adding a composite enzyme for enzymatic hydrolysis, inactivating the enzyme, filtering, and drying the filtrate to obtain enzymatic hydrolyzed lignin;

[0013] S5. Preparation of bio-based polyurethane materials: dissolve enzymatically hydrolyzed lignin in a mixed solvent, add flame-retardant aminated beads, isocyanate and initiator, stir to react, and obtain a prepolymer. Then add a chain extender, heat and stir to react, filter, wash, and dry to obtain a bio-based polyurethane material.

[0014] As a further improvement of the present invention, the mass ratio of the nano-silica microspheres and the composite aminosilane coupling agent in step S1 is 10:2-3, the temperature of the heating and stirring reaction is 40-50°C, the time is 2-3h, the average particle size range of the nano-silica microspheres is 80-120nm, and the composite aminosilane coupling agent is selected from at least two of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldiethoxysilane, and diethylenetriaminopropyltrimethoxysilane, preferably, a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2-3:7.

[0015] As a further improvement of the present invention, the mass ratio of the ammoniation beads to phosphorus oxychloride in step S2 is 10:0.15-0.3, the temperature of the heating and stirring reaction is 75-85°C, and the time is 5-7h.

[0016] As a further improvement of the present invention, the deep eutectic solvent in step S3 is prepared by mixing choline chloride, urea and ethylenediamine in a molar ratio of 1:0.7:0.3 at 65-75°C, stirring and reacting for 1-3 hours, the straw is selected from at least one of corn straw, rice straw, sorghum straw and wheat straw, the mass ratio of the straw to the deep eutectic solvent is 1:3-5, the temperature of the heating and stirring extraction is 150-170°C, and the time is 3-5 hours.

[0017] As a further improvement of the present invention, in step S4, the mass ratio of lignin to the composite enzyme is 100:3-5, the composite enzyme includes cellulase and laccase in a mass ratio of 10:3-5, the temperature of the enzymatic hydrolysis is 45-55°C, and the time is 2-4h.

[0018] As a further improvement of the present invention, the mass ratio of the enzymatic lignin, flame retardant aminated beads, isocyanate, initiator and chain extender in step S5 is 10-12:7-10:22-25:0.1-0.2:0.5-1, the initiator is dibutyltin dilaurate, the chain extender is polyethylene glycol 1000 or polyethylene glycol 2000, the mixed solvent is a mixed solution of ethanol, water, and dimethyl sulfoxide in a volume ratio of 3-5:10:2-4, the isocyanate is at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate, the stirring reaction time is 0.5-1h, the heating stirring reaction temperature is 70-80°C, and the time is 4-6h.

[0019] As a further improvement of the present invention, the present invention specifically comprises the following steps:

[0020] S1. Preparation of aminated beads: 10 parts by weight of nano-silica microspheres with an average particle size range of 80-120 nm are added to ethanol, 2-3 parts by weight of a composite aminosilane coupling agent are added, heated to 40-50°C, stirred for reaction for 2-3h, centrifuged, washed, and dried to obtain aminated beads;

[0021] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2-3:7;

[0022] S2. Preparation of flame retardant aminated pellets: 10 parts by weight of aminated pellets and 0.15-0.3 parts by weight of phosphorus oxychloride were added to ethyl acetate, heated to 75-85 ° C, stirred for 5-7h, centrifuged, washed, and dried to obtain flame retardant aminated pellets;

[0023] S3. Extraction of lignin: 10 parts by weight of straw was crushed, added to 30-50 parts by weight of a deep eutectic solvent, heated to 150-170°C, stirred and extracted for 3-5h, cooled, centrifuged, the liquid was precipitated with an equal volume of water, filtered, the solid was washed, and dried to obtain lignin;

[0024] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine in a molar ratio of 1:0.7:0.3 at 65-75° C. and stirring for 1-3 hours;

[0025] S4. Enzymatic hydrolysis of lignin: 100 parts by weight of lignin was added to water, 3-5 parts by weight of complex enzyme was added, enzymatic hydrolysis was carried out at 45-55°C for 2-4h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic lignin;

[0026] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:3-5;

[0027] S5. Preparation of bio-based polyurethane material: dissolving 10-12 parts by weight of enzymatically hydrolyzed lignin in a mixed solvent, adding 7-10 parts by weight of flame retardant aminated beads, 22-25 parts by weight of isocyanate and 0.1-0.2 parts by weight of dibutyltin dilaurate, stirring and reacting for 0.5-1h to obtain a prepolymer, then adding 0.5-1 parts by weight of a chain extender, heating to 70-80°C, stirring and reacting for 4-6h, filtering, washing, and drying to obtain a bio-based polyurethane material;

[0028] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 3-5:10:2-4.

[0029] The present invention further protects a bio-based polyurethane material prepared by the above preparation method.

[0030] The present invention further protects the use of the above bio-based polyurethane material in the preparation of waterborne polyurethane coatings.

[0031] The present invention has the following beneficial effects:

[0032] Lignin, as a renewable carbon-containing organic matter abundant in nature, contains a large number of active groups such as aromatic structures, phenolic hydroxyl groups, alcoholic hydroxyl groups, and methoxy groups. Lignin is applied to PU synthesis, which can not only reduce the consumption of petroleum resources, but also improve the mechanical properties of PU. Deep eutectic solvents have the advantages of low cost, high efficiency, simple preparation, recyclability, green and non-toxic and environmentally friendly. The deep eutectic solvents prepared by the present invention can selectively break the ether bonds between the biological straw lignin units, thereby promoting lignin cracking, and the unique strong hydrogen bonding ability can selectively crack lignin, destroy the hydrogen bonds and covalent bonds between lignin and hemicellulose, and produce low molecular weight lignin fragments, thereby greatly improving the extraction rate of lignin, while destroying the lignin macromolecular structure, breaking the unstable ether bonds between lignin molecules, and generating a large number of phenolic hydroxyl groups. The present invention further promotes the decomposition of its structure by complex enzyme hydrolysis, including cellulase and laccase, forming a large number of small molecule enzymatic hydrolysis lignins with rich hydroxyl structures. Among them, laccase can promote the adsorption between lignin and enzyme or reduce steric hindrance, thereby improving the hydrolysis efficiency of cellulase.

[0033] However, the polyurethane prepared by the reaction of the enzymatic lignin obtained by the method with isocyanate has poor mechanical properties and does not have good flame retardancy, etc. The present invention prepares flame-retardant aminated beads, and the surface of the silica nanospheres is modified by an aminosilane coupling agent, so that the surface has abundant amino groups. On the one hand, the amino groups can react with phosphorus oxychloride, so that the phosphorus oxychloride is connected to the surface of the beads, and on the other hand, the amino groups can react with isocyanate, so that the beads are coupled to the molecular chain of the polyurethane, so that the nanospheres are evenly dispersed in the polyurethane material, which greatly improves the mechanical properties and flame retardancy of the prepared bio-based polyurethane.

[0034] The bio-based polyurethane material prepared by the present invention uses agricultural byproduct straw as raw material, which greatly improves the degradability of the prepared material, reduces production costs, and improves the environmental friendliness of the material. At the same time, the prepared material has good mechanical properties and flame retardant properties, can meet industrial needs, can be used to prepare water-based polyurethane coatings, and has broad application prospects. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Nano-silica microspheres with an average particle size of 100 nm were purchased from Suzhou Beike Nanotechnology Co., Ltd. Example 1

[0037] This embodiment provides a method for preparing a bio-based polyurethane material, which specifically includes the following steps:

[0038] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 2 g of a composite aminosilane coupling agent was added, the mixture was heated to 40°C, stirred for reaction for 2 h, centrifuged, washed, and dried to obtain aminated beads;

[0039] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2:7;

[0040] S2. Preparation of flame-retardant aminated pellets: 10 g of aminated pellets and 0.15 g of phosphorus oxychloride were added to 200 mL of ethyl acetate, heated to 75 ° C, stirred for 5 h, centrifuged, washed, and dried to obtain flame-retardant aminated pellets;

[0041] S3. Lignin extraction: 10 g of straw was crushed, added to 30 g of deep eutectic solvent, heated to 150 ° C, stirred and extracted for 3 h, cooled, centrifuged, the liquid was added with an equal volume of water to precipitate for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0042] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine at a molar ratio of 1:0.7:0.3 at 65° C. and stirring for 1 hour.

[0043] S4. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 3 g of compound enzyme was added, enzymatic hydrolysis was carried out at 45 ° C for 2 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolyzed lignin;

[0044] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:3;

[0045] S5. Preparation of bio-based polyurethane material: 10 g of enzymatically hydrolyzed lignin was dissolved in 500 mL of a mixed solvent, 7 g of flame retardant aminated beads, 22 g of isocyanate and 0.1 g of dibutyltin dilaurate were added, and the mixture was stirred for 0.5 h to obtain a prepolymer, and then 0.5 g of PEG1000 was added, heated to 70 ° C, stirred for 4 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0046] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 3:10:2. Example 2

[0047] This embodiment provides a method for preparing a bio-based polyurethane material, which specifically includes the following steps:

[0048] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 3 g of a composite aminosilane coupling agent was added, the mixture was heated to 50°C, stirred for 3 h, centrifuged, washed, and dried to obtain aminated beads;

[0049] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 3:7;

[0050] S2. Preparation of flame-retardant aminated pellets: 10 g of aminated pellets and 0.3 g of phosphorus oxychloride were added to 200 mL of ethyl acetate, heated to 85 ° C, stirred for 7 h, centrifuged, washed, and dried to obtain flame-retardant aminated pellets;

[0051] S3. Lignin extraction: 10 g of straw was crushed, added to 50 g of deep eutectic solvent, heated to 170 ° C, stirred and extracted for 5 h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0052] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine in a molar ratio of 1:0.7:0.3 at 75° C. and stirring for 3 hours;

[0053] S4. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 5 g of compound enzyme was added, enzymatic hydrolysis was carried out at 55 ° C for 4 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolysis lignin;

[0054] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:5;

[0055] S5. Preparation of bio-based polyurethane material: 12 g of enzymatically hydrolyzed lignin was dissolved in 500 mL of a mixed solvent, 10 g of flame retardant aminated beads, 25 g of isocyanate and 0.2 g of dibutyltin dilaurate were added, and the mixture was stirred for 1 h to obtain a prepolymer, and then 1 g of PEG2000 was added, heated to 80 ° C, stirred for 6 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0056] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 5:10:4. Example 3

[0057] This embodiment provides a method for preparing a bio-based polyurethane material, which specifically includes the following steps:

[0058] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 2.5 g of a composite aminosilane coupling agent was added, the mixture was heated to 45°C, stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain aminated beads;

[0059] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2.5:7;

[0060] S2. Preparation of flame-retardant aminated pellets: 10 g of aminated pellets and 0.2 g of phosphorus oxychloride were added to 200 mL of ethyl acetate, heated to 80 ° C, stirred for 6 h, centrifuged, washed, and dried to obtain flame-retardant aminated pellets;

[0061] S3. Lignin extraction: 10 g of straw was crushed, added to 40 g of deep eutectic solvent, heated to 160 ° C, stirred and extracted for 4 h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0062] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine at a molar ratio of 1:0.7:0.3 at 70° C. and stirring for 2 hours;

[0063] S4. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 4 g of compound enzyme was added, enzymatic hydrolysis was carried out at 50 ° C for 3 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolyzed lignin;

[0064] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:4;

[0065] S5. Preparation of bio-based polyurethane materials: 11g of enzymatically hydrolyzed lignin was dissolved in 500mL of mixed solvent, 8.5g of flame retardant aminated beads, 23g of isocyanate and 0.15g of dibutyltin dilaurate were added, and the mixture was stirred for 1h to obtain a prepolymer. Then 0.7g of PEG1000 was added, and the mixture was heated to 75℃, stirred for 5h, filtered, washed and dried to obtain a bio-based polyurethane material. Characterization by infrared spectrum showed the following results: The peak at 3450-3300cm-1 is the absorption peak of amino group. The peak at 1410cm-1 is the characteristic vibration peak of lignin aromatic structure. The absorption peak between 1045-637cm-1 is the deformation vibration peak of aromatic C–H. 1170cm-1 is the characteristic absorption peak of P=O bond. The peaks at 2255cm-1 and 2288cm-1 are the stretching vibration peaks of free N=C=O in isocyanate. The disappearance of the peaks at 2255 cm-1 and 2270 cm-1 indicated that the functional groups in the isocyanate were consumed. The absorption intensity at 3430 cm-1 was greatly reduced, confirming that the -OH groups in lignin were consumed after the reaction with isocyanate.

[0066] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 4:10:3. Example 4

[0067] Compared with Example 3, the difference is that the complex enzyme is replaced by a single cellulase. Example 5

[0068] Compared with Example 3, the difference is that the complex enzyme is replaced by a single laccase.

[0069] Comparative Example 1

[0070] Compared with Example 3, the difference is that step S2 is not performed.

[0071] The details are as follows:

[0072] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 2.5 g of a composite aminosilane coupling agent was added, the mixture was heated to 45°C, stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain aminated beads;

[0073] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2.5:7;

[0074] S2. Lignin extraction: 10 g of straw was crushed, added to 40 g of deep eutectic solvent, heated to 160 ° C, stirred and extracted for 4 h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0075] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine at a molar ratio of 1:0.7:0.3 at 70° C. and stirring for 2 hours;

[0076] S3. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 4 g of compound enzyme was added, and the enzymatic hydrolysis was carried out at 50 ° C for 3 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolyzed lignin;

[0077] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:4;

[0078] S4. Preparation of bio-based polyurethane material: 11 g of enzymatically hydrolyzed lignin was dissolved in 500 mL of a mixed solvent, 8.5 g of aminated beads, 23 g of isocyanate and 0.15 g of dibutyltin dilaurate were added, and the mixture was stirred for 1 h to obtain a prepolymer, and then 0.7 g of PEG1000 was added, heated to 75°C, stirred for 5 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0079] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 4:10:3.

[0080] Comparative Example 2

[0081] Compared with Example 3, the difference is that the deep eutectic solvent in step S3 is replaced by water.

[0082] The details are as follows:

[0083] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 2.5 g of a composite aminosilane coupling agent was added, the mixture was heated to 45°C, stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain aminated beads;

[0084] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2.5:7;

[0085] S2. Preparation of flame-retardant aminated pellets: 10 g of aminated pellets and 0.2 g of phosphorus oxychloride were added to 200 mL of ethyl acetate, heated to 80 ° C, stirred for 6 h, centrifuged, washed, and dried to obtain flame-retardant aminated pellets;

[0086] S3. Lignin extraction: 10 g of straw was crushed, added to 40 g of water, heated to boiling, stirred and extracted for 4 h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0087] S4. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 4 g of compound enzyme was added, enzymatic hydrolysis was carried out at 50 ° C for 3 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolyzed lignin;

[0088] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:4;

[0089] S5. Preparation of bio-based polyurethane material: 11 g of enzymatically hydrolyzed lignin was dissolved in 500 mL of a mixed solvent, 8.5 g of flame retardant aminated beads, 23 g of isocyanate and 0.15 g of dibutyltin dilaurate were added, and the mixture was stirred for 1 h to obtain a prepolymer, and then 0.7 g of PEG1000 was added, heated to 75 ° C, stirred for 5 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0090] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 4:10:3.

[0091] Comparative Example 3

[0092] Compared with Example 3, the difference is that step S4 is not performed.

[0093] The details are as follows:

[0094] S1. Preparation of aminated beads: 10 g of nano-silica microspheres were added to 200 mL of ethanol, 2.5 g of a composite aminosilane coupling agent was added, the mixture was heated to 45°C, stirred for reaction for 2.5 h, centrifuged, washed, and dried to obtain aminated beads;

[0095] The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2.5:7;

[0096] S2. Preparation of flame-retardant aminated pellets: 10 g of aminated pellets and 0.2 g of phosphorus oxychloride were added to 200 mL of ethyl acetate, heated to 80 ° C, stirred for 6 h, centrifuged, washed, and dried to obtain flame-retardant aminated pellets;

[0097] S3. Lignin extraction: 10 g of straw was crushed, added to 40 g of deep eutectic solvent, heated to 160 ° C, stirred and extracted for 4 h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1 h, filtered, the solid was washed, and dried to obtain lignin;

[0098] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine at a molar ratio of 1:0.7:0.3 at 70° C. and stirring for 2 hours;

[0099] S4. Preparation of bio-based polyurethane material: 11 g of lignin was dissolved in 500 mL of mixed solvent, 8.5 g of flame retardant aminated beads, 23 g of isocyanate and 0.15 g of dibutyltin dilaurate were added, and the mixture was stirred for 1 h to obtain a prepolymer, and then 0.7 g of PEG1000 was added, heated to 75 ° C, stirred for 5 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0100] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 4:10:3.

[0101] Comparative Example 4

[0102] Compared with Example 3, the difference is that no flame retardant ammonified beads are added in step S5.

[0103] The details are as follows:

[0104] S1. Lignin extraction: 10g of straw was crushed, added to 40g of deep eutectic solvent, heated to 160°C, stirred and extracted for 4h, cooled, centrifuged, the liquid was precipitated with an equal volume of water for 1h, filtered, the solid was washed, and dried to obtain lignin;

[0105] The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine at a molar ratio of 1:0.7:0.3 at 70° C. and stirring for 2 hours;

[0106] S2. Enzymatic hydrolysis of lignin: 100 g of lignin was added to 500 mL of water, 4 g of compound enzyme was added, and the enzymatic hydrolysis was carried out at 50 ° C for 3 h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic hydrolyzed lignin;

[0107] The complex enzyme comprises cellulase and laccase in a mass ratio of 10:4;

[0108] S3. Preparation of bio-based polyurethane material: 19.5 g of enzymatically hydrolyzed lignin was dissolved in 500 mL of a mixed solvent, 23 g of isocyanate and 0.15 g of dibutyltin dilaurate were added, and the mixture was stirred for 1 h to obtain a prepolymer, and then 0.7 g of PEG1000 was added, the mixture was heated to 75°C, stirred for 5 h, filtered, washed, and dried to obtain a bio-based polyurethane material;

[0109] The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 4:10:3.

[0110] Test Example 1

[0111] The bio-based polyurethane materials prepared in Examples 1-5 and Comparative Examples 1-4 were evenly coated using a coating machine, with a coating amount of 10 g / m2.

[0112] Tensile index: The tensile index was measured using a tensile tester according to ISO 1924-2:2008.

[0113] Tear index: The tear index was measured using a tear tester according to ISO 1974:2012.

[0114] Degradability: buried in natural soil, depth of 10cm. Soil environment temperature is between 12℃ and 28℃, humidity fluctuates between 30% and 60%. Morphological observation is carried out on the 14th day, and its degradation rate is calculated, degradation rate (%) = (m0-m1) / m0. Among them, m0 is the initial mass of the film, and m1 is the mass of the film after being buried in the soil for 14 days.

[0115] Flexibility: The flexibility of the coating film is measured using the national standard GB / T 1731-1993 "Determination of paint film flexibility";

[0116] Flame retardant time: The flame retardant time is determined according to the national standard GB 12441-2005 "Surface fire retardant coatings".

[0117] The results are shown in Table 1.

[0118] Table 1

[0119]

[0120] It can be seen from the above table that the bio-based polyurethane materials prepared in Examples 1-3 of the present invention have good mechanical properties, flexibility, flame retardancy and biodegradability.

[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a bio-based polyurethane material, characterized in that: The following steps are involved: S1. Preparation of aminated beads: adding nano-silica microspheres to ethanol, adding a composite aminosilane coupling agent, heating and stirring to react, centrifuging, washing, and drying to obtain aminated beads; the mass ratio of the nano-silica microspheres to the composite aminosilane coupling agent is 10:2-3, the temperature of the heating and stirring reaction is 40-50°C, the time is 2-3h, and the average particle size of the nano-silica microspheres is in the range of 80-120nm; S2. Preparation of flame retardant aminated pellets: The aminated pellets and phosphorus oxychloride were added to ethyl acetate, heated and stirred to react, centrifuged, washed, and dried to obtain flame retardant aminated pellets; S3. Extraction of lignin: The straw is crushed, added to a deep eutectic solvent, heated and stirred for extraction, cooled, centrifuged, the liquid is precipitated with water, filtered, the solid is washed, and dried to obtain lignin; S4. Enzymatic hydrolysis of lignin: adding lignin to water, adding a composite enzyme for enzymatic hydrolysis, inactivating the enzyme, filtering, and drying the filtrate to obtain enzymatic hydrolyzed lignin; S5. Preparation of bio-based polyurethane material: dissolving enzymatically hydrolyzed lignin in a mixed solvent, adding flame retardant aminated beads, isocyanate and dibutyltin dilaurate, stirring to react, preparing a prepolymer, then adding a chain extender, heating and stirring to react, filtering, washing, and drying to prepare a bio-based polyurethane material; The deep eutectic solvent in step S3 is prepared by mixing choline chloride, urea and ethylenediamine in a molar ratio of 1:0.7:0.3 at 65-75°C and stirring for 1-3h; the mass ratio of the straw to the deep eutectic solvent is 1:3-5, and the temperature of the heating and stirring extraction is 150-170°C for 3-5h; In step S4, the mass ratio of lignin to the composite enzyme is 100:3-5, the composite enzyme includes cellulase and laccase in a mass ratio of 10:3-5, the temperature of the enzymolysis is 45-55° C., and the time is 2-4 h.

2. The preparation method according to claim 1, characterized in that: The composite aminosilane coupling agent in step S1 is selected from at least two of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldiethoxysilane, and diethylenetriaminopropyltrimethoxysilane.

3. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the ammoniation beads to phosphorus oxychloride is 10:0.15-0.3, the temperature of the heating and stirring reaction is 75-85° C., and the time is 5-7 hours.

4. The preparation method according to claim 1, characterized in that: The straw is selected from at least one of corn straw, rice straw, sorghum straw and wheat straw.

5. The preparation method according to claim 1, characterized in that: In step S5, the mass ratio of enzymatic lignin, flame retardant aminated beads, isocyanate, dibutyltin dilaurate and chain extender is 10-12:7-10:22-25:0.1-0.2:0.5-1, the chain extender is polyethylene glycol 1000 or polyethylene glycol 2000, the mixed solvent is a mixed solution of ethanol, water and dimethyl sulfoxide in a volume ratio of 3-5:10:2-4, the isocyanate is toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate at least one, the stirring reaction time is 0.5-1h, the heating stirring reaction temperature is 70-80°C, and the time is 4-6h.

6. The preparation method according to claim 1, characterized in that: The specific steps include: S1. Preparation of aminated beads: 10 parts by weight of nano-silica microspheres with an average particle size range of 80-120 nm are added to ethanol, 2-3 parts by weight of a composite aminosilane coupling agent are added, heated to 40-50°C, stirred for reaction for 2-3h, centrifuged, washed, and dried to obtain aminated beads; The composite aminosilane coupling agent is a mixture of γ-aminopropyltrimethoxysilane and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, with a mass ratio of 2-3:7; S2. Preparation of flame retardant aminated pellets: 10 parts by weight of aminated pellets and 0.15-0.3 parts by weight of phosphorus oxychloride were added to ethyl acetate, heated to 75-85 ° C, stirred for 5-7h, centrifuged, washed, and dried to obtain flame retardant aminated pellets; S3. Extraction of lignin: 10 parts by weight of straw was crushed, added to 30-50 parts by weight of a deep eutectic solvent, heated to 150-170°C, stirred and extracted for 3-5h, cooled, centrifuged, the liquid was precipitated with an equal volume of water, filtered, the solid was washed, and dried to obtain lignin; The deep eutectic solvent is prepared by mixing choline chloride, urea and ethylenediamine in a molar ratio of 1:0.7:0.3 at 65-75° C. and stirring for 1-3 hours; S4. Enzymatic hydrolysis of lignin: 100 parts by weight of lignin was added to water, 3-5 parts by weight of complex enzyme was added, enzymatic hydrolysis was carried out at 45-55°C for 2-4h, the enzyme was inactivated, filtered, and the filtrate was dried to obtain enzymatic lignin; The complex enzyme comprises cellulase and laccase in a mass ratio of 10:3-5; S5. Preparation of bio-based polyurethane material: dissolving 10-12 parts by weight of enzymatically hydrolyzed lignin in a mixed solvent, adding 7-10 parts by weight of flame retardant aminated beads, 22-25 parts by weight of isocyanate and 0.1-0.2 parts by weight of dibutyltin dilaurate, stirring and reacting for 0.5-1h to obtain a prepolymer, then adding 0.5-1 parts by weight of a chain extender, heating to 70-80°C, stirring and reacting for 4-6h, filtering, washing, and drying to obtain a bio-based polyurethane material; The mixed solvent is a mixture of ethanol, water and dimethyl sulfoxide in a volume ratio of 3-5:10:2-4.

7. A bio-based polyurethane material obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the bio-based polyurethane material as claimed in claim 7 in the preparation of waterborne polyurethane coatings.

Citation Information

Patent Citations

  • Laccase activated and modified sulfonated soda lignin amphiphilic polymer and preparation method and application thereof

    CN102199268A

  • Flame-retardant modified silane coupling agent and preparation method thereof

    CN103570758A

  • Bio-based polyurethane elastomer and preparation method thereof

    CN115073697A

Cited By

  • Bio-based polyurethane foaming thermal insulation material and preparation method thereof

    CN121851692A