Ferromanganese phosphate precursor, lithium iron manganese phosphate and preparation method and application thereof
The co-precipitation method is used to prepare ammonium manganese phosphate and deaminating ammonia to form ferromanganese phosphate. Combined with lithium salt sintering, the problems of uneven element distribution and high energy consumption in the synthesis of positive electrode materials of lithium-ion batteries are solved, and high purity and low The cost of lithium manganese iron phosphate material improves electrochemical performance and safety.
Patent Information
- Application Number
- CN202411146592.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The synthesis method of the existing lithium-ion battery cathode material lithium manganese iron phosphate has problems such as uneven element distribution, poor structural stability, high energy consumption, high cost and safety, and the use of alkaline hazardous chemicals is not conducive to industrial promotion.
The divalent ferromanganese phosphate precursor ammonium manganese phosphate is prepared by co-precipitation method, and the divalent ferromanganese phosphate is dehydrated and dehydrated by deamination, and mixed with lithium salt to sinter, avoid the use of alkaline hazardous chemicals, and improve elemental uniformity and electrochemistry. Performance, reduce costs and energy consumption.
It realizes the preparation of lithium manganese iron phosphate materials with high purity, low impurity and low cost, improves electrochemical performance and energy density, simplifies the process flow, and improves safety and reproducibility.
Smart Images

Figure CN118666263B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery positive electrode materials, and in particular relates to a manganese iron phosphate precursor, lithium manganese iron phosphate, and a preparation method and application thereof. Background Art
[0002] At present, lithium-ion batteries are the mainstream power batteries, and their cathode materials mainly use lithium iron phosphate, ternary materials, lithium cobalt oxide, lithium manganese oxide, etc. Among them, lithium manganese iron phosphate (LMFP) is widely used in lithium-ion battery cathodes due to its advantages of low cost, high safety, long cycle life, high voltage and wide source of raw materials. It has the advantages of both the excellent rate performance of lithium iron phosphate and the high voltage platform of lithium manganese phosphate, and has gradually become an advanced choice to replace lithium iron phosphate, and will become an important choice in the future new energy vehicle and energy storage market.
[0003] Some studies have mixed lithium sources, phosphorus sources, iron oxides, manganese oxides, etc. and sintered them to obtain LMFP through a solid-phase route. The element distribution is uneven, the ratio uniformity is poor, the structural stability is poor, and the battery capacity, rate and other electrical properties are poor. Some studies have used a wet co-precipitation method to prepare a trivalent manganese iron phosphate precursor, which is then mixed with a lithium source and roasted to obtain LMFP. The trivalent manganese iron phosphate precursor has poor process reproducibility and high energy consumption, which is not conducive to large-scale production. In addition, a reducing agent is required in the subsequent roasting process to reduce the Mn and Fe elements, which increases costs and reduces energy density. Ammonium manganese iron phosphate contains three elements, Fe, Mn, and P. Both Mn and Fe are divalent, have a suitable stoichiometric ratio and stable physical and chemical properties, and are ideal precursors for preparing lithium manganese iron phosphate.
[0004] The synthesis methods of LMFP positive electrode materials mainly include high-temperature solid-phase method and liquid-phase method. The liquid-phase method mainly includes hydrothermal method and co-precipitation method. The solid-phase method mainly involves solid-phase mixing of lithium source, manganese source, iron source and phosphorus source, and then sintering at high temperature to form lithium manganese iron phosphate, while the liquid-phase method mainly involves uniformly mixing soluble raw materials in a solution and then synthesizing the product. Although the solid-phase method is simple, elements such as Mn and Fe cannot be uniformly mixed at the atomic level, and it is difficult to evenly distribute them in the main structure of LMFP, resulting in Mn 3+The Jahn-Teller effect is serious, which affects the cycle stability and rate performance of the battery. The liquid phase synthesis of lithium manganese iron phosphate can improve the uniformity of transition metals in LMFP, but the hydrothermal method requires a high temperature and high pressure environment, and has high requirements for production equipment. There are problems such as cumbersome production operations, poor safety, high energy consumption and low production capacity. The co-precipitation method first uses a wet method to synthesize a manganese iron phosphate precursor, and then mixes it with a lithium source for sintering. The conditions of this synthesis route are mild, and the elements of the prepared product are evenly distributed and the proportions are precisely adjustable. It is currently a popular route. The co-precipitation method has two route precursors: divalent and trivalent. The trivalent manganese iron phosphate precursor route requires the metal to be oxidized to form manganese iron phosphate, and then the reducing agent is consumed in subsequent use for reduction. The process has poor reproducibility and is not conducive to large-scale production.
[0005] The invention patent with the authorization announcement number CN 118004990B discloses a ferromanganese phosphate precursor, lithium iron manganese phosphate and a preparation method thereof. The preparation method of the ferromanganese phosphate precursor is: stirring at high speed in a reactor, adding a first mixed solution, a supplementary precipitant and a first doping additive in succession to perform a synthetic reaction to obtain a ferromanganese phosphate co-precipitate, filtering, washing and drying the slurry containing the ferromanganese phosphate co-precipitate to obtain a ferromanganese phosphate precursor, wherein the supplementary precipitant is ammonium bicarbonate or baking soda, and the first doping additive is a titanium sulfate solution. The preparation method of lithium iron manganese phosphate is: adding a ferromanganese phosphate precursor, a lithium source, a carbon source, a second doping additive and water to a reactor to obtain a slurry; grinding, spray drying, high-temperature sintering and crushing the slurry to obtain lithium iron manganese phosphate with a particle size D50 of 0.8~1.5μm, wherein the second doping additive is magnesium oxide, which can ultimately improve the processing consistency and electrochemical performance of lithium iron manganese phosphate. However, this method uses alkaline hazardous chemicals such as ammonium bicarbonate or baking soda in the process of preparing ferromanganese phosphate precursor, and requires the additional addition of a phosphorus source. The use of a supplementary precipitant and a first doping additive will introduce impurities, which is not conducive to the industrial promotion and application of the preparation process.
[0006] The patent application with application publication number CN 117886296A discloses an ammonium manganese ferrophosphate, a lithium manganese ferrophosphate and a preparation method and application thereof. Through the corrosion reaction of iron powder and manganese powder in water, the hydrolysis reaction of ammonium ions and the regulation of the pH of the reaction system by ammonia water, the metal ions in the solution react with NH3 and PO4 3-Combined to form ammonium manganese iron phosphate, Fe and Mn can be completely converted into the product to achieve uniform mixing of Fe, Mn, and P at the atomic level, and the ammonium ions in the reaction solution can be recycled, greatly improving the atomic economy; the ammonium manganese iron phosphate is calcined to obtain hydrogen manganese iron phosphate, and then calcined with a lithium source and a carbon source to finally obtain a lithium manganese iron phosphate material with spherical secondary particles, high purity, high tap density, nanometer-scale particle size and uniform distribution, and good discharge specific capacity and rate performance. When applied to lithium-ion batteries, it can improve the electrochemical performance of lithium-ion batteries. However, this method uses alkaline hazardous chemicals such as ammonia water in the process of preparing ammonium manganese iron phosphate, which is not conducive to the industrialization and promotion of the preparation process. Summary of the invention
[0007] Based on the shortcomings of the prior art, the present invention provides a ferromanganese phosphate precursor, lithium ferromanganese phosphate and a preparation method thereof. The method first adopts a coprecipitation method to prepare a divalent ferromanganese phosphate precursor, ammonium ferromanganese phosphate, which is then roasted, dehydrated and deaminated to generate hydrogen manganese phosphate, and then the hydrogen manganese phosphate and lithium salt are mixed and sintered to form LMFP. In the preparation process of ammonium ferromanganese phosphate, no alkaline hazardous chemicals such as ammonia water, ammonium bicarbonate, sodium bicarbonate, etc. are used. Only manganese salts, iron salts and phosphate salts necessary to form the substance are used. No other additional impurity elements need to be introduced during the coprecipitation process. The obtained product has a high purity and a low impurity content. The process is simple and practical, with good reproducibility, and the atoms are evenly dispersed, and finally a single crystal phase precursor compound ammonium ferromanganese phosphate with uniform morphology is formed. In the process of preparing hydrogen manganese ferrophosphate by deammoniation and dehydration of ammonium manganese ferrophosphate, the first carbon source and ammonium manganese ferrophosphate are mixed and roasted, which can effectively avoid the oxidation of elements such as Mn and Fe. In the subsequent preparation stage of lithium manganese ferrophosphate, carbon and other elements that enhance the conductivity of the material are introduced in advance, which can effectively improve the electrochemical properties of the material such as capacity and rate. At the same time, the amount of inert gas such as nitrogen can be greatly reduced, the operation safety can be improved, the cost can be reduced, and the volatile ammonia can be recycled and reused to achieve green production. Finally, hydrogen manganese ferrophosphate is roasted with the lithium source and the second carbon source, and the final lithium manganese ferrophosphate has high purity, low cost, high compaction density, good electrochemical properties such as capacity and rate, and ideal energy density.
[0008] The present invention adopts the following technical solution to solve the above technical problems, and the preparation method of ferromanganese phosphate precursor comprises the following specific preparation steps:
[0009] Step S1, respectively preparing a manganese-iron mixed solution, a first precipitant solution, and a second precipitant solution, wherein the manganese salt in the manganese-iron mixed solution is one or more of manganese sulfate, manganese nitrate, manganese chloride, or manganese acetate, the iron salt is one or more of ferrous sulfate, ferrous nitrate, or ferrous chloride, the first precipitant is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or ammonium phosphate, and the second precipitant is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, or potassium dihydrogen phosphate;
[0010] Step S2, adding pure water and the first precipitant solution into the reactor, adding the manganese iron mixed solution prepared in step S1, the first precipitant solution and the second precipitant solution into the reactor in parallel under stirring conditions, controlling the pH of the reaction system to be 4.0-6.5 by adjusting the feeding rate of the second precipitant solution, stopping the addition of liquid after the reaction time reaches the requirement, performing solid-liquid separation on the reaction materials, washing with pure water and then drying to obtain a single crystalline compound ammonium manganese iron phosphate.
[0011] It is further defined that the total concentration of manganese salt and iron salt in the manganese-iron mixed solution in step S1 is 0.5-3.0 mol / L; the concentration of the first precipitant in the first precipitant solution is 0.5-3.0 mol / L; the concentration of the second precipitant in the second precipitant solution is 0.5-3.0 mol / L.
[0012] It is further defined that the rotation speed of the reactor in step S2 is 200-1000 r / min, and the temperature of the reactor is 30-80°C.
[0013] It is further defined that the feeding rate of the manganese-iron mixed solution in step S2 is 1000-3000 mL / min, and the feeding rate of the first precipitant solution is 500-5000 mL / min.
[0014] The ferromanganese phosphate precursor of the present invention is a single crystalline compound ammonium ferromanganese phosphate with uniform morphology, and its molecular formula is NH4Mn x Fe y PO4, where x+y=1, 0.01<x≤0.99, 0.01<y≤0.99, the manganese iron ammonium phosphate atoms are evenly distributed, and the specific surface area is 1-25m 2 / g, sulfur content ≤800ppm, (Mn+Fe) / P molar ratio is 0.96-1.04.
[0015] The preparation method of lithium manganese iron phosphate described in the present invention comprises the following specific preparation steps:
[0016] Step S1, mixing the prepared ammonium manganese ferrous phosphate with a first carbon source, wherein the first carbon source is one or more of ascorbic acid, glucose, sucrose, fructose, ribose, polyethylene glycol (PEG), polyvinyl alcohol (PVA) or citric acid, and calcining at 300-400° C. for 3-6 hours to perform deamination and dehydration to obtain hydrogen manganese ferrophosphate, and the removed ammonia is recovered and repeatedly recycled;
[0017] Step S2, mixing the manganese iron hydrogen phosphate obtained in step S1 with a lithium salt and a second carbon source, wherein the molar ratio of the raw materials satisfies Li: (Mn + Fe) is (0.8-1.5): 1, and the second carbon source is starch, phenolic resin, soybean lecithin, ascorbic acid, glucose, sucrose, fructose, ribose, polyethylene glycol (PEG), polyvinyl alcohol (PVA) or citric acid. One or more of the mixture is sand milled, spray dried, and then calcined at 550-900 ° C for 5-15h to obtain high-purity lithium manganese iron phosphate.
[0018] Further defined, the molecular formula of the manganese ferrophosphate in step S1 is Mn x Fe y HPO4, where x+y=1, 0.01<x≤0.99, 0.01<y≤0.99.
[0019] It is further defined that the lithium salt in step S2 is one or more of lithium carbonate and lithium hydroxide.
[0020] It is further defined that the amount of the first carbon source in step S1 is 50wt%-90wt% of the total carbon amount, the amount of the second carbon source in step S2 is 10wt%-50wt% of the total carbon amount, and the total carbon amount in the lithium manganese iron phosphate is 1wt%-5wt%.
[0021] The lithium manganese iron phosphate described in the present invention is used as a positive electrode material for preparing a button-type lithium-ion battery.
[0022] The present invention synthesizes a single crystalline compound ammonium manganese iron phosphate with controllable specific surface area, sulfur, morphology, particle size and other indicators and uniform element distribution by wet coprecipitation of phosphate, manganese salt, iron salt and the like, then mixes the ammonium manganese iron phosphate with a first carbon source and calcines to obtain hydrogen manganese iron phosphate, and finally calcines hydrogen manganese iron phosphate with a lithium salt and a second carbon source to obtain high-purity lithium manganese iron phosphate with high compaction density and excellent electrical properties such as capacity and rate. The present invention has the following advantages and beneficial effects:
[0023] 1) In the preparation process of ammonium manganese ferric phosphate, only the necessary manganese salt, iron salt and phosphate salt are used to form the substance. No alkaline hazardous chemicals such as ammonia water, ammonium bicarbonate, sodium bicarbonate, etc. are used. At the same time, no other additional impurity elements need to be introduced. The product has high purity and low content of impurities such as sulfur. The process is simple and practical, with good reproducibility, uniform atomic dispersion, good processing performance, and a specific surface area of 1-25m2 / g is adjustable, the sulfur content is ≤800ppm, the (Mn+Fe) / P molar ratio is 0.97-1.02, and finally a single crystalline phase compound ammonium manganese iron phosphate with uniform morphology is obtained.
[0024] 2) In the process of deamination and dehydration of ammonium ferric manganese phosphate to prepare hydrogen manganese ferrophosphate, the first carbon source and ammonium ferric manganese phosphate are mixed and roasted, which can effectively avoid the oxidation of elements such as Mn and Fe. In the preparation stage of lithium manganese ferrophosphate, elements such as carbon that enhance the conductivity of the material are introduced in advance, which effectively improves the electrochemical properties of the material such as capacity and rate. At the same time, it can greatly reduce the use of inert gases such as nitrogen, improve operational safety, reduce costs, and recover and reuse the volatilized ammonia to achieve green production and further reduce costs.
[0025] 3) The preparation process of lithium manganese iron phosphate divalent manganese iron phosphate precursor is simple and reproducible. A large flow process is used to increase production capacity and further reduce production costs.
[0026] 4) By utilizing the reducing properties and conductivity of the carbon source at the same time, a portion of the carbon source is introduced when preparing manganese hydrogen ferrophosphate, and a small portion of the carbon source is introduced when preparing lithium manganese iron phosphate, which is beneficial to improving electrochemical properties such as capacity and rate, reducing the use of inert gas, increasing compaction density, and increasing energy density. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the SEM image of ammonium manganese ferrous phosphate prepared in Example 1.
[0028] Figure 2 This is the EDS-mapping diagram of ammonium manganese ferrous phosphate prepared in Example 1.
[0029] Figure 3 This is the SEM image of ammonium manganese ferrous phosphate prepared in Example 2
[0030] Figure 4 This is the SEM image of ammonium manganese ferrous phosphate prepared in Comparative Example 1. DETAILED DESCRIPTION
[0031] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0032] Step S1, preparing a manganese-iron mixed solution with a total concentration of 2.0 mol / L using manganese sulfate and ferrous sulfate, preparing a first precipitant solution with a concentration of 2.0 mol / L using ammonium dihydrogen phosphate, and preparing a second precipitant solution with a concentration of 2.0 mol / L using diammonium hydrogen phosphate.
[0033] Step S2, adding pure water and 100% of the experimental amount of the first precipitant solution into the reactor, setting the speed of the reactor to 1000 r / min and the temperature of the reactor to 40°C.
[0034] Step S3, adding the manganese-iron mixed solution at a feeding rate of 3000 mL / min and the first precipitant at a feeding rate of 3000 mL / min to the reactor in parallel, and at the same time adding the second precipitant solution to the reactor at a certain feeding rate, and controlling the pH of the reaction system to 4.2-4.3 by adjusting the feeding rate of the second precipitant solution.
[0035] Step S4, after reacting for 30 minutes, stop feeding the liquid, separate the reaction material into solid and liquid and wash it with pure water, the pure water temperature is 25°C, and obtain a single crystalline compound ammonium manganese iron phosphate NH4Mn 0.6 Fe 0.4 PO4, the atoms are evenly distributed (e.g. Figure 1 As shown), good processing performance, specific surface area of 10.14m 2 / g, the sulfur content is 524ppm, and the (Mn+Fe) / P molar ratio is 0.99.
[0036] Step S5, mixing ammonium manganese ferrous phosphate with glucose accounting for 70 wt% of the total carbon dosage, roasting at 380° C. for 3 h to deaminate and dehydrate to obtain hydrogen manganese ferrophosphate, and recovering the removed ammonia for reuse.
[0037] Step S6, mixing manganese iron hydrogen phosphate with lithium carbonate and citric acid accounting for 30wt% of the total carbon content, wherein the molar ratio of each raw material satisfies Li:(Mn+Fe) of 1.05:1, sand grinding, spray drying, and then roasting at 800°C for 6h. The cooled material is sieved with a 325-mesh ultrasonic vibration screen to obtain high-purity lithium manganese iron phosphate, wherein the total carbon content of the lithium manganese iron phosphate is 2wt%.
[0038] The lithium manganese iron phosphate is used as the positive electrode material to be assembled into a CR2016 button battery. The first discharge capacity at 0.1C is 158mAh / g, and at a high rate of 1C, the first cycle discharge capacity is 149mAh / g. Example 2
[0039] Step S1, prepare a manganese-iron mixed solution with a total concentration of 3.0 mol / L using manganese acetate and ferrous sulfate, prepare a first precipitant solution with a total concentration of 3.0 mol / L using ammonium dihydrogen phosphate and diammonium hydrogen phosphate, and prepare a second precipitant solution with a concentration of 2.0 mol / L using ammonium phosphate.
[0040] Step S2, adding pure water and 50% of the experimental amount of the first precipitant solution into the reactor, setting the speed of the reactor to 400 r / min and the temperature of the reactor to 70°C.
[0041] Step S3, adding the manganese-iron mixed solution at a feeding rate of 1000 mL / min and the first precipitant solution at a feeding rate of 800 mL / min to the reactor in parallel, and at the same time adding the second precipitant solution to the reactor at a certain feeding rate, and controlling the pH of the reaction system to 6.1-6.2 by adjusting the feeding rate of the second precipitant solution.
[0042] Step S4, after reacting for 60 minutes, stop feeding the liquid, separate the reaction material into solid and liquid and wash it with pure water, the pure water temperature is 60°C, and obtain a single crystalline compound ammonium manganese iron phosphate NH4Mn 0.6 Fe 0.4 PO4, the atoms are evenly distributed (e.g. Figure 2 As shown), good processing performance, specific surface area of 20.88m 2 / g, the sulfur content is 435ppm, and the (Mn+Fe) / P molar ratio is 0.98.
[0043] Step S5, mixing ammonium manganese ferrous phosphate with glucose accounting for 80 wt% of the total carbon dosage, roasting at 320° C. for 4 h to deaminate and dehydrate to obtain hydrogen manganese ferrophosphate, and recovering the removed ammonia for repeated recycling.
[0044] Step S6, mixing manganese iron hydrogen phosphate with lithium carbonate and sucrose accounting for 20wt% of the total carbon content, wherein the molar ratio of each raw material satisfies Li: (Mn + Fe) of 1.2: 1, sand milling, spray drying, and then roasting at 600° C. for 10 h. The cooled material is sieved with a 325-mesh ultrasonic vibration screen to obtain high-purity lithium manganese iron phosphate, wherein the total carbon content of the lithium manganese iron phosphate is 1wt%.
[0045] The lithium manganese iron phosphate is used as the positive electrode material to be assembled into a CR2016 button battery. The first discharge capacity at 0.1C is 163mAh / g, and at a high rate of 1C, the first cycle discharge capacity is 154mAh / g.
[0046] Comparative Example 1
[0047] Step S1, preparing a manganese-iron mixed solution with a total concentration of 2.0 mol / L using manganese sulfate and ferrous sulfate, and preparing a precipitant solution with a concentration of 2.0 mol / L using ammonium dihydrogen phosphate.
[0048] Step S2, adding pure water into the reactor, setting the rotation speed of the reactor to 1000 r / min, and the temperature of the reactor to 40°C.
[0049] Step S3, adding the manganese-iron mixed solution at a feeding rate of 3000mL / min and the precipitant solution at a feeding rate of 3000mL / min to the reactor in parallel, and adding ammonia water with a concentration of 8mol / L to the reactor in parallel at a certain rate, and controlling the pH of the reaction system to 4.2-4.3 by adjusting the feeding rate of ammonia water.
[0050] Step S4, after reacting for 30 minutes, stop feeding the liquid, separate the reaction material into solid and liquid and wash it with pure water, the pure water temperature is 25°C, to obtain ammonium manganese iron phosphate NH4Mn 0.6 Fe 0.4 PO4, the atoms are unevenly distributed (e.g. Figure 4 As shown), the sheet is thick, the processing performance is poor, and the specific surface area is 0.33m 2 / g, the sulfur content is 1800ppm, and the (Mn+Fe) / P molar ratio is 1.05.
[0051] Step S5, calcining ammonium manganese ferrophosphate at 380° C. for 3 h in a nitrogen atmosphere to remove ammonia and water to obtain hydrogen manganese ferrophosphate, and recovering the removed ammonia for repeated recycling.
[0052] Step S6, mixing manganese iron hydrogen phosphate with lithium carbonate and glucose, wherein the molar ratio of each raw material satisfies Li: (Mn + Fe) of 1.05: 1, sand grinding, spray drying, and then roasting at 800 ° C for 6 hours. The cooled material is sieved with a 325-mesh ultrasonic vibration screen to obtain lithium manganese iron phosphate, and the total carbon content of the lithium manganese iron phosphate is 2wt%.
[0053] The lithium manganese iron phosphate is used as the positive electrode material to be assembled into a CR2016 button battery. The first discharge capacity at 0.1C is 142mAh / g, and at a high rate of 1C, the first cycle discharge capacity is 131mAh / g.
[0054] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing lithium manganese iron phosphate, characterized in that The specific preparation steps are: Step S1, respectively preparing a manganese-iron mixed solution, a first precipitant solution, and a second precipitant solution, wherein the manganese salt in the manganese-iron mixed solution is one or more of manganese sulfate, manganese nitrate, manganese chloride, or manganese acetate, the iron salt is one or more of ferrous sulfate, ferrous nitrate, or ferrous chloride, the first precipitant is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or ammonium phosphate, and the second precipitant is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, or potassium dihydrogen phosphate; Step S2, adding pure water and the first precipitant solution into the reaction kettle, adding the manganese iron mixed solution prepared in step S1, the first precipitant solution and the second precipitant solution into the reaction kettle in parallel under stirring conditions, controlling the pH of the reaction system to be 4.0-6.5 by adjusting the feeding rate of the second precipitant solution, stopping the addition of liquid after the reaction time reaches the requirement, performing solid-liquid separation on the reaction materials, washing with pure water and then drying to obtain a single crystalline compound of manganese iron ammonium phosphate; Step S3, mixing the ammonium manganese ferrous phosphate prepared in step S2 with a first carbon source, wherein the first carbon source is one or more of ascorbic acid, glucose, sucrose, fructose, ribose, polyethylene glycol, polyvinyl alcohol or citric acid, and calcining at 300-400° C. for 3-6 hours to perform deamination and dehydration to obtain hydrogen manganese ferrophosphate, and the removed ammonia is recovered and repeatedly recycled; Step S4, mixing the manganese iron hydrogen phosphate obtained in step S3 with a lithium salt and a second carbon source, wherein the molar ratio of the raw materials satisfies Li: (Mn + Fe) is (0.8-1.5): 1, and the second carbon source is starch, phenolic resin, soybean lecithin, ascorbic acid, glucose, sucrose, fructose, ribose, polyethylene glycol (PEG), polyvinyl alcohol (PVA) or citric acid. One or more of the mixture is sand milled, spray dried, and then calcined at 550-900 ° C for 5-15h to obtain high-purity lithium manganese iron phosphate.
2. The method for preparing lithium iron manganese phosphate according to claim 1, characterized in that: The total concentration of manganese salt and iron salt in the manganese-iron mixed solution in step S1 is 0.5-3.0 mol / L; the concentration of the first precipitant in the first precipitant solution is 0.5-3.0 mol / L; the concentration of the second precipitant in the second precipitant solution is 0.5-3.0 mol / L.
3. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: In step S2, the rotation speed of the reactor is 200-1000 r / min, and the temperature of the reactor is 30-80°C.
4. The method for preparing lithium iron manganese phosphate according to claim 1, characterized in that: In step S2, the feeding rate of the ferromanganese mixed solution is 1000-3000 mL / min, and the feeding rate of the first precipitant solution is 500-5000 mL / min.
5. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: The ammonium manganese iron phosphate in step S2 is a single crystalline compound with uniform morphology, and its molecular formula is NH4Mn x Fe y PO4, where x+y=1, 0.01<x≤0.99, 0.01<y≤0.99, the manganese iron ammonium phosphate atoms are evenly distributed, and the specific surface area is 1-25m 2 / g, sulfur content ≤800ppm, (Mn+Fe) / P molar ratio is 0.96-1.
04.
6. The method for preparing lithium iron manganese phosphate according to claim 1, characterized in that: The molecular formula of the manganese ferrophosphate in step S3 is Mn x Fe y HPO4, where x+y=1, 0.01<x≤0.99, 0.01<y≤0.
99.
7. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: The lithium salt in step S4 is one or more of lithium carbonate and lithium hydroxide.
8. The lithium iron manganese phosphate prepared according to the method of claim 1 is used as a positive electrode material to prepare a button-type lithium-ion battery.
Citation Information
Patent Citations
Manganese iron ammonium phosphate, manganese iron lithium phosphate, and preparation method and application of manganese iron ammonium phosphate and manganese iron lithium phosphate
CN117886296A
Ferromanganese phosphate precursor, lithium iron manganese phosphate and preparation method thereof
CN118004990B
Lithium manganese iron phosphate precursor, lithium manganese iron phosphate positive electrode material, preparation method of lithium manganese iron phosphate positive electrode material, electrode material, electrode and lithium ion battery
CN113942990A
Cited By
Manganese iron phosphate precursor and lithium manganese iron phosphate, and preparation methods therefor and use thereof
EP4725900A1
Manganese iron phosphate precursor and lithium manganese iron phosphate, and preparation methods therefor and use thereof
WO2026040398A1