A reservoir bottom film with a width of not less than 6m and its preparation process
By using chlorinated polyethylene, thermoplastic polyolefin and other components in the bottom film of the warehouse and the melt extrusion process, the problems of limited width and high splicing cost of the bottom film of the warehouse are solved, and an ultra-wide width with high toughness and waterproof performance is achieved. The preparation of the bottom film of the library extends the service life and reduces the cost.
Patent Information
- Application Number
- CN202411162331.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The width of the existing warehouse bottom film is limited, and the splicing cost of ultra-wide warehouse bottom films is high and prone to cracks, which affects the performance and service life.
Using components such as chlorinated polyethylene, thermoplastic polyolefin, ethylene-vinyl acetate copolymer, plasticizer, carbon black, stabilizer and lubricant, a warehouse bottom with a width of not less than 6m is prepared through melt mixing and extrusion processes. Membrane, increase the toughness and waterproof performance of the material, reduce melt viscosity, improve adhesion and reduce air spots and ripples.
It has realized the preparation of warehouse bottom membrane with a width of not less than 6m, improved the toughness and mechanical properties of the material, ensured the ultra-wide waterproof performance, extended the service life and reduced the cost.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of membrane materials, and in particular to a reservoir bottom membrane with a width of not less than 6m and a preparation process thereof. Background Art
[0002] As a special structure, seepage in water conservancy projects not only wastes water resources, but also affects the stability of the dam. As a new type of artificial synthetic polymer material, reservoir bottom membrane has good toughness, deformation resistance and ductility, which can help the dam withstand certain compressive stress and improve the stability of the dam.
[0003] However, the current reservoir bottom membranes are limited to narrow widths, and there are few wide width products. The super-wide reservoir bottom membranes used in super-large venues are often spliced together by multiple narrow width reservoir bottom membranes. Although the splicing can meet the anti-seepage function of the reservoir bottom membrane to a certain extent, the cost is high. After long-term use, cracks will appear at the splicing under the action of external forces, and water seepage may occur, which will affect the performance of the material and reduce its service life. Summary of the invention
[0004] The inventors have found that the width of existing reservoir bottom membranes is generally within 6m. If the width of the reservoir bottom membrane is to be increased, it is necessary to improve the plasticity and toughness of the material to a certain extent to solve the problem of air spots and flow lines easily generated on the surface of ultra-wide reservoir bottom membranes, while ensuring the waterproofness of the reservoir bottom membrane.
[0005] In order to solve the above problems, the present invention provides a reservoir bottom film with a width of not less than 6m. The reservoir bottom film comprises the following components by weight: 50-70 parts of chlorinated polyethylene, 30-50 parts of thermoplastic polyolefin, 10-20 parts of ethylene-vinyl acetate copolymer, 20-30 parts of plasticizer, 2-10 parts of carbon black, 5-10 parts of stabilizer and 10-15 parts of lubricant.
[0006] Thermoplastic polyolefin is a blend of thermoplastic hard polymer material and thermosetting rubber polymer, wherein the mass fraction of the thermosetting rubber polymer accounts for more than 50%.
[0007] On the other hand, the present invention provides a preparation process for a bottom film with a width of not less than 6m, and the preparation process comprises the following steps: the raw materials are melt-mixed in proportion at 150°C-200°C, the materials are melt-plasticized and extruded to a tee through an extruder, the materials enter a spiral flow channel through a vertically upward discharge hole through the tee, and then extruded in the form of a tube embryo through a straight portion through the gap between the core mold and the mouth, the molten tube embryo is inflated into a film tube by compressed air, and the film product is cooled, pulled and rolled up.
[0008] Among them, the draft ratio is (30-60):1.
[0009] Compared with the prior art, the present invention achieves at least one of the following beneficial effects:
[0010] (1) The bottom film of the present invention with a width of not less than 6m adopts chlorinated polyethylene and thermoplastic polyolefin, and adds additives such as carbon black, stabilizer, plasticizer, lubricant, etc., and provides a bottom film with a width of not less than 6m through compounding of a series of raw materials. The ultra-wide bottom film can promote the good dispersion of thermoplastic polyolefin in chlorinated polyethylene by adding an appropriate amount of ethylene-vinyl acetate copolymer. In addition, in order to improve the width and adhesion, the addition of plasticizer can reduce the melt viscosity of the material to a certain extent, but it will reduce the flexibility of the bottom film material to a certain extent, resulting in material fracture. By adding thermoplastic polyolefin, the toughness of the material can be improved, and at the same time, it is not easy to produce air spots and flow lines on the surface.
[0011] (2) A waterproofing agent is added to the reservoir bottom membrane with a width of not less than 6 m for modification. Maleic anhydride in the waterproofing agent is a polar substance. It can be grafted onto the polyethylene wax molecular chain under the action of diisopropylbenzene peroxide. The obtained waterproofing agent has both polar and non-polar groups. The polar group can react with the polar group in chlorinated polyethylene, and the non-polar group has good compatibility with thermoplastic polyolefins. It can be compounded with other fillers to improve the toughness and mechanical properties of the reservoir bottom membrane, so that the prepared reservoir bottom membrane can ensure ultra-wide width while having good waterproof performance.
[0012] (3) Organic silicone is added to the reservoir bottom membrane with a width of not less than 6 m of the present invention. During the preparation of the reservoir bottom membrane, other inorganic fillers are coated in the organic silicone in a nucleation structure, and the organic silicone at the other end is combined with chlorinated polyethylene and embedded in the thermoplastic polyolefin structure, which can not only connect inorganic substances, but also fuse chlorinated polyethylene and thermoplastic polyolefin, promote the dispersion of fillers, enhance toughness, and further improve the lubricity of chlorinated polyethylene, making the surface of the reservoir bottom membrane smoother, laying a foundation for expanding the width of the reservoir bottom membrane.
[0013] (4) In the preparation process of the base film with a width of not less than 6m of the present invention, in order to ensure that the ultra-wide base film has good mechanical properties and the lateral strength of the base film, the draft ratio is set to 30-60:1. In addition, the molten material enters the spiral flow channel through the vertical upward discharge hole from the tee and performs an upward spiral motion, which can greatly reduce the phenomenon of uneven melt caused by uneven heating and ensure the mechanical properties of the base film. DETAILED DESCRIPTION
[0014] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below in an illustrative manner in conjunction with the specification.
[0015] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and therefore, the scope of protection of the present invention is not limited by the specific embodiments disclosed below. In the description of this specification, the description of reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily have to be directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0016] In an exemplary embodiment of the present invention, the bottom film with a width of not less than 6 m includes the following components: 50-70 parts of chlorinated polyethylene, 30-50 parts of thermoplastic polyolefin, 10-20 parts of ethylene-vinyl acetate copolymer, 20-30 parts of plasticizer, 2-10 parts of carbon black, 5-10 parts of stabilizer and 10-15 parts of lubricant;
[0017] Thermoplastic polyolefin is a blend of thermoplastic hard polymer material and thermosetting rubber polymer, wherein the mass fraction of the thermosetting rubber polymer accounts for more than 50%.
[0018] Optionally, the mass ratio of chlorinated polyethylene to thermoplastic polyolefin is (1.8-2):1. Furthermore, a single chlorinated polyethylene bottom film has excellent properties, such as good permeability resistance and good low-temperature flexibility, but it also has certain defects. In actual use, narrow bottom films are usually spliced together, and chlorinated polyethylene bottom films are prone to local bulging and low tear strength, so that water seepage occurs during long-term use. In order to solve the above problems, the inventors have found through repeated studies that thermoplastic polyolefins have good high and low temperature resistance and excellent weather resistance. Starting from raw materials, the present invention uses chlorinated polyethylene and thermoplastic polyolefins, adds additives such as carbon black, stabilizers, plasticizers, lubricants, etc., and provides a bottom film with a width of not less than 6m through the compounding of a series of raw materials. The ultra-wide bottom film can promote the good dispersion of thermoplastic polyolefins in chlorinated polyethylene by adding an appropriate amount of ethylene-vinyl acetate copolymer. In addition, in order to increase the width and improve the adhesion, adding plasticizers can reduce the melt viscosity of the material to a certain extent, but it will reduce the flexibility of the bottom film material to a certain extent, causing the material to break. By adding thermoplastic polyolefins, the toughness of the material can be improved, and at the same time, it is not easy to produce air spots and flow lines on the surface.
[0019] Optionally, the mass fraction of the thermosetting rubber polymer is more than 70%; the thermosetting rubber polymer is EPDM and / or EPDM; the thermoplastic hard polymer material is polyethylene and / or polypropylene. Preferably, the mass fraction of the thermosetting rubber polymer is 70%-80%, ensuring that the prepared bottom membrane has good toughness and flexibility.
[0020] Optionally, the invention further comprises 5-15 parts of a waterproofing agent, wherein the preparation method of the waterproofing agent comprises the following steps: uniformly mixing polyethylene wax, maleic anhydride and dicumyl peroxide, and performing banburying at 80-150° C. to obtain the waterproofing agent. The mass ratio of polyethylene wax, maleic anhydride and dicumyl peroxide is (90-99): (0.2-2): (0.2-3).
[0021] Optionally, the mass ratio of polyethylene wax, maleic anhydride and diisopropylbenzene peroxide is (95-98): (0.5-1): (0.5-1.5). Preferably, the mass ratio of polyethylene wax, maleic anhydride and diisopropylbenzene peroxide is 98:1:1. Furthermore, during the preparation process, polyethylene wax can improve the dispersion of fillers in the polymer, and its non-polar molecular chain has good compatibility with chlorinated polyethylene and thermoplastic polyolefins. Maleic anhydride is a polar substance, which can be grafted onto the polyethylene wax molecular chain under the action of diisopropylbenzene peroxide. The resulting waterproofing agent has both polar and non-polar groups. The polar group can react with the polar group in the chlorinated polyethylene, and the non-polar group has good compatibility with thermoplastic polyolefins, which can improve the toughness and mechanical properties of the reservoir bottom film, so that the prepared reservoir bottom film can ensure ultra-wide width while having good waterproof performance.
[0022] Optionally, 3-5 parts of carbon black, and the average particle size of carbon black is less than 30nm. Carbon black within this range can ensure the mechanical properties of the reservoir bottom membrane and ensure that the system has a relatively uniform elastic network structure.
[0023] Optionally, the plasticizer is one or more of dioctyl phthalate, chlorinated paraffin, epoxidized soybean oil, and dibutyl phthalate.
[0024] Preferably, the plasticizer is a compound of chlorinated paraffin, dibutyl phthalate and epoxidized soybean oil. Specifically, by mass fraction, chlorinated paraffin accounts for 50%-70%, phthalic acid accounts for 15-25%, and epoxidized soybean oil accounts for 15-30%. The compounded plasticizer compound can promote the dispersion of fillers such as carbon black, thereby ensuring the mechanical properties of the bottom film.
[0025] Optionally, the lubricant is a compound of talcum powder and polyethylene wax; wherein the mass ratio of talcum powder to polyethylene wax is 1:2-4.
[0026] Preferably, the mass ratio of talc to polyethylene wax is 1:2.5.
[0027] Optionally, 10-20 parts of organic silicone are also included. Preferably, 13-17 parts of organic silicone are included. Further, organic silicone, also known as siloxane or polysiloxane, is an elemental organic polymer with -Si-O- chain as the main chain and -CH3 as the side chain, and has a similar structure to the PP polymer with -CC- chain as the main chain, and the side chains all contain -CH3 groups. In the process of preparing the bottom film of the reservoir, other inorganic fillers are coated in the organic silicone with a nucleation structure, and the organic silicone at the other end is combined with chlorinated polyethylene and embedded in the thermoplastic polyolefin structure, which can not only connect inorganic substances, but also fuse chlorinated polyethylene and thermoplastic polyolefin, promote the dispersion of fillers, enhance toughness, and further improve the lubricity of chlorinated polyethylene, making the surface of the bottom film of the reservoir smoother.
[0028] Optionally, the stabilizer is one or more of 2,6-di-tert-butyl-4-methylphenol, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (referred to as antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol (referred to as antioxidant 1076), and diisooctyl phenyl phosphite.
[0029] In another exemplary embodiment of the present invention, the preparation process of the bottom film with a width of not less than 6m includes the following steps: the raw materials are melt-mixed in proportion at 150°C-200°C, the materials are melt-plasticized and extruded to a tee through an extruder, and enter the spiral flow channel through the tee through a vertically upward discharge hole, and then extruded in the shape of a tube embryo through a straight portion and the gap between the core mold and the mouth, the molten tube embryo is inflated into a film tube by compressed air, and is cooled, pulled and rolled into a film product.
[0030] Among them, the draft ratio is (30-60):1. To further explain, the draft ratio refers to the ratio of the film tube speed when passing through the nip roller to the tube embryo extrusion speed. As the material draft ratio increases, the tear strength of the bottom film decreases. In order to ensure that the ultra-wide bottom film has good mechanical properties and the lateral strength of the bottom film, the draft ratio is set to 30-60:1. In addition, the molten material enters the spiral flow channel through the vertical upward discharge hole from the tee and performs an upward spiral motion, which can greatly reduce the phenomenon of uneven melt caused by uneven heating and ensure the mechanical properties of the bottom film.
[0031] Optionally, a co-rotating twin-screw extruder is selected to blend and extrude the premix. The twin-screw extruder heats the equipment during processing. Each heating zone is a partition. Different processing temperatures are set for each partition according to different processing technologies. At the same time, the barrel screw elements corresponding to each partition are also different. During processing, it can be divided into 4 to 6 zones, each zone includes 2 to 4 sub-zones, and the processing temperature in the same sub-zone is uniform and unchanged. The processing temperature of each zone increases in sequence. The material is evenly dispersed and the performance of each material is fully utilized. For example, the processing temperatures of zones 1 to 12 of the above-mentioned twin-screw extruder can be: 160°C in zone 1, 160°C in zone 2, 160°C in zone 3, 160°C in zone 4, 170°C in zone 5, 170°C in zone 6, 180°C in zone 7, 180°C in zone 8, 185°C in zone 9, 185°C in zone 10, 200°C in zone 11, and 200°C in zone 12.
[0032] Example 1
[0033] The 7m wide bottom film includes the following components: 50 parts of chlorinated polyethylene, 30 parts of thermoplastic polyolefin, 10 parts of ethylene-vinyl acetate copolymer, 20 parts of plasticizer, 2 parts of carbon black, with an average particle size of 40nm, 5 parts of stabilizer and 10 parts of lubricant. Among them, the thermoplastic polyolefin is a mixture of 60% EPDM rubber and 40% polyethylene; the plasticizer is a compound of chlorinated paraffin and epoxidized soybean oil, with chlorinated paraffin accounting for 70% and epoxidized soybean oil accounting for 30%; the lubricant is a compound of talc and polyethylene wax in a mass ratio of 1:2, and the stabilizer is 2,6-di-tert-butyl-4-methylphenol.
[0034] The preparation process of the bottom film with a width of 7m includes the following steps: adding the above raw materials to a high-speed blender in proportion, stirring to obtain a premix, selecting a co-rotating twin-screw extruder to blend and extrude the premix, and the processing temperatures of zones 1 to 12 of the twin-screw extruder can be respectively: zone 1 160°C, zone 2 160°C, zone 3 160°C, zone 4 160°C, zone 5 170°C, zone 6 170°C, zone 7 180°C, zone 8 180°C, zone 9 185°C, zone 10 185°C, zone 11 200°C, zone 12 200°C. The material is melted and plasticized by the extruder and extruded to the tee, and then enters the spiral flow channel through the vertical upward discharge hole of the tee, and then extruded from the gap between the core mold through a straight section in the shape of a tube embryo, and the molten tube embryo is inflated into a film tube by compressed air, and then cooled, pulled and rolled into a film product. Among them, the draft ratio is 30:1.
[0035] The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine. The screw temperatures of zones 1 to 4 of the blow molding machine are 180°C, 185°C, 190°C, and 200°C, respectively. The bottom film is obtained by blow molding and winding.
[0036] Example 2
[0037] The 7.5m wide bottom film includes the following components: 65 parts of chlorinated polyethylene, 35 parts of thermoplastic polyolefin, 15 parts of ethylene-vinyl acetate copolymer, 25 parts of plasticizer, 3 parts of carbon black, with an average particle size of 20nm, 7 parts of stabilizer, 12 parts of lubricant, 8 parts of waterproofing agent and 12 parts of organic silicone. Among them, the thermoplastic polyolefin is a mixture of 70% EPDM rubber and 30% polyethylene; the plasticizer is a compound of chlorinated paraffin, dibutyl phthalate and epoxidized soybean oil, with chlorinated paraffin accounting for 50%, epoxidized soybean oil accounting for 25%, and phthalic acid accounting for 25%; the lubricant is a compound of talc and polyethylene wax in a mass ratio of 1:2.5, and the stabilizer is a compound of 2,6-di-tert-butyl-4-methylphenol and antioxidant 1076.
[0038] The preparation method of the waterproofing agent comprises the following steps: uniformly mixing polyethylene wax, maleic anhydride and dicumyl peroxide in a mass ratio of 98:1:1, and performing banburying at 100 DEG C to obtain the waterproofing agent.
[0039] The preparation process of the 7.5m wide bottom film includes the following steps: adding the above raw materials to a high-speed blender in proportion, stirring to obtain a premix, selecting a co-rotating twin-screw extruder to blend and extrude the premix, and the processing temperatures of zones 1 to 12 of the twin-screw extruder can be: zone 1 160°C, zone 2 160°C, zone 3 165°C, zone 4 165°C, zone 5 170°C, zone 6 170°C, zone 7 175°C, zone 8 175°C, zone 9 180°C, zone 10 180°C, zone 11 185°C, zone 12 185°C. The material is melted and plasticized by the extruder and extruded to the tee, and then enters the spiral flow channel through the vertical upward discharge hole of the tee, and then extruded from the gap of the core mold through a straight section in the shape of a tube embryo, and the molten tube embryo is inflated into a film tube by compressed air, and then cooled, pulled and rolled into a film product. Among them, the draft ratio is 40:1.
[0040] The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine. The screw temperatures of zones 1 to 4 of the blow molding machine are 170°C, 180°C, 185°C, and 190°C, respectively. The bottom film is obtained by blow molding and winding.
[0041] Example 3
[0042] The 8m wide bottom film includes the following components: 70 parts of chlorinated polyethylene, 50 parts of thermoplastic polyolefin, 20 parts of ethylene-vinyl acetate copolymer, 30 parts of plasticizer, 7 parts of carbon black, with an average particle size of 25nm, 10 parts of stabilizer, 15 parts of lubricant, 12 parts of waterproof agent and 20 parts of organic silicone. Among them, the thermoplastic polyolefin is a mixture of 70% EPDM rubber and 30% polypropylene; the plasticizer is a compound of chlorinated paraffin, dibutyl phthalate and epoxidized soybean oil, with chlorinated paraffin accounting for 70%, epoxidized soybean oil accounting for 15%, and phthalic acid accounting for 15%; the lubricant is a compound of talc and polyethylene wax in a mass ratio of 1:2.5, and the stabilizer is a compound of 2,6-di-tert-butyl-4-methylphenol and antioxidant 1010.
[0043] The preparation method of the waterproofing agent comprises the following steps: uniformly mixing polyethylene wax, maleic anhydride and dicumyl peroxide in a mass ratio of 95:2:3, and performing banburying at 80 DEG C to obtain the waterproofing agent.
[0044] The preparation process of the 8m wide bottom film includes the following steps: adding the above raw materials to a high-speed blender in proportion, stirring to obtain a premix, selecting a co-rotating twin-screw extruder to blend and extrude the premix, and the processing temperatures of zones 1 to 12 of the twin-screw extruder can be: zone 1 160°C, zone 2 160°C, zone 3 165°C, zone 4 165°C, zone 5 170°C, zone 6 170°C, zone 7 175°C, zone 8 175°C, zone 9 180°C, zone 10 180°C, zone 11 185°C, zone 12 185°C. The material is melted and plasticized by the extruder and extruded to the tee, and then enters the spiral flow channel through the vertical upward discharge hole of the tee, and then extruded from the gap of the core mold through a straight section in the shape of a tube embryo, and the molten tube embryo is inflated into a film tube by compressed air, and then cooled, pulled and rolled into a film product. Among them, the draft ratio is 50:1.
[0045] The pellets obtained by extrusion are placed in a three-layer co-extrusion blow molding machine. The screw temperatures of zones 1 to 4 of the blow molding machine are 170°C, 180°C, 185°C, and 190°C, respectively. The bottom film is obtained by blow molding and winding.
[0046] Example 4
[0047] Based on Example 2, the main difference is that the plasticizer is a compound of chlorinated paraffin, dioctyl phthalate and epoxidized soybean oil.
[0048] Example 5
[0049] The main difference between the above two embodiments is that no waterproofing agent is added.
[0050] Example 6
[0051] The main difference from Example 2 is that no organic silicone is added.
[0052] Example 7
[0053] Based on Example 2, the main difference is that the width of the bottom membrane is 10m.
[0054] Comparative Example 1
[0055] Based on Example 1, the main difference is that the mass fraction of the thermosetting rubber polymer accounts for 30%.
[0056] Comparative Example 2
[0057] The main difference from Example 1 is that no thermoplastic polyolefin is added.
[0058] Comparative Example 3
[0059] The main difference is that no ethylene-vinyl acetate copolymer is added based on Example 1.
[0060] The bottom membranes prepared in Examples 1-7 and Comparative Examples 1-3 were subjected to performance tests. The thickness of the bottom membranes was 2 mm, and the tensile strength and elongation at break were tested in accordance with GB / T17632 and GB / T1040.2-2006; the angular tear strength was tested in accordance with GB / T17632 and QB / T1130, with a test speed of 200 mm / min; the puncture resistance was tested in accordance with GB / T17632 and Appendix D of GB / T17643-2011, with a test speed of 300 mm / min; the anti-seepage performance was tested in accordance with GB / T17632 and GB / T328.10, and the test results are shown in Table 1.
[0061] Table 1
[0062]
[0063] As shown in Table 1, it can be seen that the bottom film prepared by the present invention has good mechanical properties. The elongation at break is not less than 850%, the tensile strength is not less than 50 kN / m, the transverse right-angle tear load is not less than 320 N, the longitudinal right-angle tear load is not less than 340 N, the puncture resistance is not less than 600 N, there is no leakage at 0.3 MPa ≥ 24 h, and it has good waterproof performance.
[0064] In addition, the surface of the reservoir bottom membrane with a width of not less than 6 m prepared by the present invention is not prone to air spots, flow lines and the like.
[0065] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A bottom film with a width of not less than 6m, characterized in that: The bottom film comprises the following components by weight: 50-70 parts of chlorinated polyethylene, 30-50 parts of thermoplastic polyolefin, 10-20 parts of ethylene-vinyl acetate copolymer, 20-30 parts of plasticizer, 2-10 parts of carbon black, 5-10 parts of stabilizer and 10-15 parts of lubricant; Thermoplastic polyolefin is a mixture of thermoplastic hard polymer material and thermosetting rubber polymer, wherein the mass fraction of the thermosetting rubber polymer accounts for more than 50%; The thermosetting rubber polymer is EPDM rubber and / or EPDM rubber; The thermoplastic hard polymer material is polyethylene and / or polypropylene.
2. The bottom film of the reservoir according to claim 1, characterized in that: The mass ratio of chlorinated polyethylene to thermoplastic polyolefin is (1.8-2):
1.
3. The bottom film of the reservoir according to claim 1, characterized in that: The mass fraction of the thermosetting rubber polymer is more than 70%.
4. The bottom film of the reservoir according to claim 1, characterized in that: It also includes a waterproofing agent, and the preparation method of the waterproofing agent includes the following steps: The polyethylene wax, maleic anhydride and dicumyl peroxide are uniformly mixed and mixed at 80-150° C. to obtain a waterproofing agent; Wherein, the mass ratio of polyethylene wax, maleic anhydride and diisopropylbenzene peroxide is (90-99): (0.2-2): (0.2-3).
5. The bottom film of the reservoir according to claim 4, characterized in that: The mass ratio of polyethylene wax, maleic anhydride and dicumyl peroxide is 98:1:
1.
6. The bottom film of the reservoir according to claim 1, characterized in that: 3-5 parts of carbon black, with an average particle size of less than 30nm.
7. The bottom film of the reservoir according to claim 1, characterized in that: The plasticizer is one or more of dioctyl phthalate, chlorinated paraffin, epoxidized soybean oil, and dibutyl phthalate.
8. The bottom film of the reservoir according to claim 1, characterized in that: The lubricant is a compound of talcum powder and polyethylene wax; wherein the mass ratio of talcum powder to polyethylene wax is 1:2-4.
9. The bottom film of the reservoir according to claim 1, characterized in that: It also includes 10-20 parts of organic silicone.
10. A process for preparing a bottom film with a width of not less than 6 m as claimed in any one of claims 1 to 9, characterized in that: The preparation process comprises the following steps: melt-mixing the raw materials at 150° C.-200° C. in proportion, melting and plasticizing the materials through an extruder and extruding them to a tee, and then entering a spiral flow channel through a vertically upward discharge hole from the tee, and then extruding them through a straight section through a gap between a core die and a mouth in the shape of a tube embryo, and blowing the molten tube embryo into a film tube through compressed air, and then cooling, pulling and rolling them into a film product; Among them, the draft ratio is (30-60):1.
Citation Information
Patent Citations
Formula and production method for shoe material, and production method for secondarily molded sole
CN106939097A
Anti-permeation geomembrane for dam and preparation method of anti-permeation geomembrane
CN115674852A