In-situ complexation ultraviolet absorption high-weather-resistance protective coating and preparation method thereof
By using in-situ complexed UV absorbers in concrete protective coatings, the problem of UV absorber agglomeration is solved, the UV absorption rate and the durability of the coating are improved, and the service life of the concrete structure is extended.
Patent Information
- Application Number
- CN202411152481.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
UV absorbers such as zinc oxide and titanium dioxide powder directly added to existing concrete protective coatings are prone to agglomeration, resulting in a decrease in UV absorption rate, coating deterioration and shortened service life.
Metal oxide nanoparticles are reacted with N,N-dimethylformamide to generate an active precursor, which is then hydrothermally reacted with polyvinyl alcohol aqueous solution to form an in-situ complexed UV absorber. The complexation reaction forms a stable borate ester structure to avoid agglomeration and improve uniform dispersion.
It increases the UV absorption rate, enhances the UV aging resistance of the coating, provides good waterproof and anti-permeability effects and bonding strength, and extends the service life of the concrete structure.
Smart Images

Figure CN118725167A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete protective coatings, and in particular to an in-situ complexed ultraviolet absorption high weather resistance protective coating and a preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Highway bridge concrete anti-collision guardrails are widely used in my country's highway bridge construction due to their excellent protective performance. However, in areas with heavy snowfall in winter, such as northern my country and plateau areas, concrete anti-collision guardrail diseases are also increasing day by day, such as cracking and peeling of the concrete surface, and corrosion of steel bars. These diseases not only affect the appearance of concrete guardrails, but also affect the anti-collision ability, increasing safety hazards. Concrete protective coating is a means to effectively improve the durability of concrete. The coating can form a waterproof barrier on the concrete surface, blocking moisture and harmful substances from entering the concrete, and preventing concrete from being corroded by chloride ions, damage from freeze-thaw cycles, and carbonization.
[0004] However, long-term exposure of the concrete surface to ultraviolet radiation will cause photochemical reactions, resulting in coating degradation and shedding. In addition, long-term exposure to ultraviolet rays will also cause fading and yellowing of the coating, affecting the appearance. The addition of functional fillers such as ultraviolet absorbers can effectively alleviate the above problems, improve the weather resistance of the coating, prevent its premature aging and failure, thereby better protecting the concrete from environmental factors and extending the service life of the concrete structure. At present, common ultraviolet absorbing materials mainly include zinc oxide, titanium dioxide powder, etc. However, these materials have a large specific surface area and surface energy, and are not dispersible. They are prone to agglomeration when directly added to the coating material, and cannot form a uniform and stable dispersion state, resulting in a decrease in the effective filling amount and ultraviolet absorption rate of the ultraviolet absorbing material in the coating. Summary of the invention
[0005] In view of the above problems, the present invention provides an in-situ complexed ultraviolet absorption high weather resistance protective coating and a preparation method thereof, wherein the prepared ultraviolet absorption material can be evenly dispersed in the coating system, thereby improving the ultraviolet absorption rate of the coating. Specifically, the present invention discloses the following technical solutions.
[0006] In a first aspect, the present invention provides an ultraviolet absorber, the structural formula of which is shown in formula (1): Formula (1).
[0007] In the above formula (1), M includes at least one of metal elements such as Zn, Ti, and Sn.
[0008] In a second aspect, the present invention provides a method for preparing the ultraviolet absorber, comprising the steps of: (1) Mix metal oxide (MO) nanoparticles and N,N-dimethylformamide (DMF) and heat them to react. After the reaction is completed, separate the solid product to obtain the active precursor (M-DMF) for later use.
[0009] (2) A polyvinyl alcohol (PVA) aqueous solution and the active precursor are mixed and subjected to a hydrothermal reaction. After completion, a solid product is separated to obtain a UV absorber (PVA@M-DMF).
[0010] Furthermore, in step (1), the mass ratio of the metal oxide (MO) nanoparticles to N,N-dimethylformamide is 20-40:55-75. Optionally, the metal oxide (MO) includes at least one of ZnO, TiO2, SnO2, etc.
[0011] Furthermore, in step (1), the heating temperature is 95-145°C, the reaction time is 90-150 min, and the shear rate is 400-800 r / min. Preferably, continuous stirring is performed during the reaction. In this process, the N,N-dimethylformamide (DMF) is first adsorbed on the surface of the MO, and then the carbon-hydrogen bonds of the DMF are activated and broken under high temperature and high-speed shearing conditions, and the hydrogen element is replaced by the more active zinc element, and a dehydration condensation reaction occurs to form the active precursor (M-DMF). The reaction process is shown in formula (2): Formula (2).
[0012] Furthermore, in step (2), the mass fraction of the polyvinyl alcohol aqueous solution is 2-5%.
[0013] Furthermore, in step (2), the mass ratio of the polyvinyl alcohol aqueous solution to the active precursor is 30-60:40-70.
[0014] Furthermore, in step (2), the temperature of the hydrothermal reaction is 170-240°C, the pressure is 0.35-0.75 MPa, and the time is 45 min-110 min. In this process, the high pressure and high temperature provided by the hydrothermal reaction increase the bond energy of the carbon-oxygen double bond in the active precursor (M-DMF), which then breaks to form two single-bonded carbon atoms and one single-bonded oxygen atom. The single-bonded oxygen atom combines with another single-bonded oxygen atom provided by PVA to form a stable COOC structure, thereby obtaining a UV absorber (PVA@M-DMF). The reaction process is shown in formula (3): Formula (3).
[0015] In a third aspect, the present invention discloses an in-situ complexed ultraviolet absorption concrete protective coating, which comprises the following raw materials in parts by weight: Component A comprises 16-38 parts of glass powder, 25-45 parts of silicon powder, 35-52 parts of talc powder, 2-8 parts of borate ion source, and 1-4 parts of solid additive. Component B comprises 48-68 parts of polymer emulsion, 13-25 parts of ultraviolet absorber (PVA@M-DMF), 8-16 parts of water, and 1-3 parts of liquid additive. Wherein: the ultraviolet absorber is as shown in the above formula (1).
[0016] Furthermore, the mass ratio of component A to component B is 30-60:30-60.
[0017] Furthermore, the borate ion source includes at least one of borax, boric acid, etc.
[0018] Further, the solid additive includes at least one of a defoamer, a water reducer, etc. Optionally, the mass ratio of the defoamer to the water reducer is 60-80:15-30. Optionally, the defoamer includes at least one of a polyether polymer defoamer, an organosilicon defoamer, etc. The water reducer includes at least one of a polycarboxylic acid water reducer, a naphthalene water reducer, etc.
[0019] Further, the liquid auxiliary agent includes at least one of a film-forming auxiliary agent, a dispersant, etc. Optionally, the mass ratio of the film-forming auxiliary agent to the dispersant is 0.5-2:2-5. Optionally, the film-forming auxiliary agent includes at least one of polyvinyl pyrrolidone, phenoxy propanol, etc. The dispersant includes at least one of sodium tripolyphosphate, sodium hexametaphosphate, etc.
[0020] Further, the polymer emulsion includes at least one of ethylene-vinyl acetate (VAE) emulsion, acrylic acid ester (PA) emulsion, etc. Optionally, the solid content of the polymer emulsion ranges from 40% to 60%.
[0021] In a fourth aspect, the present invention discloses a method for preparing the in-situ complexing ultraviolet absorption concrete protective coating, comprising the following steps: uniformly mixing the component A and the component B to obtain the coating.
[0022] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects: Traditionally, when ultraviolet absorbers such as zinc oxide and titanium dioxide powder are directly added to concrete protective coatings, they are prone to agglomeration and cannot form a uniform and stable dispersion state, resulting in a decrease in the ultraviolet absorption rate of the ultraviolet absorber in the coating. In addition, the agglomeration of ultraviolet absorber particles will also cause weak areas of ultraviolet absorption in the coating, which will cause the coating to deteriorate first from these weak areas of ultraviolet absorption and lose its protective effect. In addition, if the ultraviolet absorbing particles agglomerate severely, it will also cause defects in the coating system, which will directly lead to the degradation of the mechanical properties of the coating and shorten its life.
[0023] To this end, the present invention provides a metal polymer ultraviolet absorber as shown in the above formula (1). This ultraviolet absorber utilizes its alcoholic hydroxyl group and undergoes an in-situ complexation reaction with the borate ion provided by the B component. That is, as shown in formula (4), the hydroxyl group in the borate ion is replaced by the alcoholic hydroxyl group of the ultraviolet absorber to form a borate ester complex. This in-situ complexed ultraviolet absorber is stabilized by the formation of a boron-oxygen bond. This is because the formation of the boron-oxygen bond is that the borate ion and the hydroxyl group are fully coordinated and replaced by the alcoholic hydroxyl group of the ultraviolet absorber to form a borate ester complex, which eliminates the problem of easy agglomeration of the ultraviolet absorbing material itself and greatly improves its uniform dispersibility, thereby reducing the agglomeration phenomenon of the ultraviolet absorber after entering the concrete protective coating, so that it can be more evenly dispersed in the coating, and the ultraviolet absorption rate is improved. At the same time, the above-mentioned complexation reaction can also form an ultra-dense, highly flexible three-dimensional cross structure with the polymer emulsion, so that the coating has good waterproof and anti-seepage effects while being resistant to ultraviolet aging, and has high bonding strength and high elongation at break, thereby improving the service life: Formula (4). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0025] Figure 1 A sample diagram of the UV absorber prepared in Example 1 below; Figure 2 The following is a SEM image of the UV absorber prepared in Example 1. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0027] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions.
[0028] In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The technical solution of the present invention is further described in conjunction with the accompanying drawings and specific embodiments.
[0029] Example 1 1. A method for preparing an ultraviolet absorber, comprising the following steps: (1) ZnO nanoparticles and N,N-dimethylformamide (DMF) were mixed in a mass ratio of 32:68, heated in a water bath to 120°C, and stirred at a rate of 500 r / min for 120 min. After completion, the solid product was filtered out to obtain the active precursor (Zn-DMF) for later use.
[0030] (2) A 3% polyvinyl alcohol (PVA) aqueous solution and the active precursor were mixed at a mass ratio of 45:55, and then magnetically stirred at a speed of 600 r / min for 30 minutes. After completion, the mixture was placed in a high-temperature and high-pressure reactor, and the reactor temperature was set to 200°C, the pressure was set to 0.5 MPa, and the reaction time was set to 90 minutes. After completion, the solid product was filtered out to obtain a UV absorber (PVA@Zn-DMF), such as Figure 1 shown.
[0031] 2. A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating, comprising the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 20 parts of glass powder, 32 parts of silicon powder, 43 parts of filling-grade talc, 2.5 parts of borax, and 2.5 parts of solid additives. The solid additives are composed of an organosilicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 78:22.
[0032] Component B is formed by mixing 52 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 55%, 18 parts of PVA@Zn-DMF of this embodiment, 12 parts of water, and 1.5 parts of a liquid additive, wherein the liquid additive is composed of a film-forming aid (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 1:3.
[0033] (2) The above-mentioned component A and component B are mixed in a mass ratio of 50:50 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0034] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0035] Example 2 1. A method for preparing an ultraviolet absorber, comprising the following steps: (1) TiO2 nanoparticles and N,N-dimethylformamide (DMF) were mixed in a mass ratio of 20:75, heated in a water bath to 95°C, and stirred at a rate of 400 r / min for 150 min. After completion, the solid product was filtered out to obtain the active precursor (Ti-DMF) for later use.
[0036] (2) A 2% polyvinyl alcohol (PVA) aqueous solution and the active precursor were mixed at a mass ratio of 60:40, and then magnetically stirred at a speed of 600 r / min for 30 minutes. After completion, the mixture was placed in a high-temperature and high-pressure reactor, the reactor temperature was set to 170°C, the pressure was set to 0.75 MPa, and the reaction time was set to 110 minutes. After completion, the solid product was filtered out to obtain a UV absorber (PVA@Ti-DMF).
[0037] 2. A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating, comprising the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 38 parts of glass powder, 45 parts of silicon micropowder, 52 parts of filling-grade talc, 8 parts of borax, and 4 parts of solid additives. The solid additives are composed of an organic silicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 60:30.
[0038] Component B is formed by mixing 68 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 40%, 25 parts of PVA@Ti-DMF of this embodiment, 16 parts of water, and 3 parts of a liquid additive, wherein the liquid additive is composed of a film-forming aid (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 0.5:2.
[0039] (2) The above-mentioned component A and component B are mixed in a mass ratio of 30:60 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0040] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0041] Example 3 1. A method for preparing an ultraviolet absorber, comprising the following steps: (1) SnO2 nanoparticles and N,N-dimethylformamide (DMF) were mixed in a mass ratio of 40:55, heated in a water bath to 145°C, and stirred at a rate of 800 r / min for 90 min. After completion, the solid product was filtered out to obtain the active precursor (Sn-DMF) for later use.
[0042] (2) A 5% polyvinyl alcohol (PVA) aqueous solution and the active precursor were mixed at a mass ratio of 30:70, and then magnetically stirred at a speed of 600 r / min for 25 minutes. After completion, the mixture was placed in a high-temperature and high-pressure reactor, the reactor temperature was set to 240°C, the pressure was set to 0.35 MPa, and the reaction time was set to 45 minutes. After completion, the solid product was filtered out to obtain a UV absorber (PVA@Sn-DMF).
[0043] 2. A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating, comprising the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 16 parts of glass powder, 25 parts of silicon micropowder, 35 parts of filling-grade talc, 2 parts of boric acid, and 1 part of solid additive. The solid additive is composed of a polyether polymer defoamer and a polycarboxylic acid water reducer in a mass ratio of 80:15.
[0044] Component B is formed by mixing 48 parts of acrylate (PA) emulsion with a solid content of 60%, 13 parts of PVA@Sn-DMF of this embodiment, 8 parts of water, and 1 part of a liquid additive, wherein the liquid additive is composed of a film-forming aid (phenoxypropanol) and a dispersant (sodium hexametaphosphate) in a mass ratio of 2:5.
[0045] (2) The above-mentioned component A and component B are mixed in a mass ratio of 60:30 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0046] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0047] Example 4 A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating comprises the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 20 parts of glass powder, 32 parts of silicon powder, 43 parts of filling-grade talc, 2.5 parts of borax, and 2.5 parts of solid additives. The solid additives are composed of an organosilicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 78:22.
[0048] Component B is formed by mixing 52 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 55%, 18 parts of the active precursor (Zn-DMF) prepared in the above embodiment, 12 parts of water, and 1.5 parts of a liquid additive, wherein the liquid additive is composed of a film-forming additive (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 1:3.
[0049] (2) The above-mentioned component A and component B are mixed in a mass ratio of 50:50 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0050] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0051] Example 5 A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating comprises the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 20 parts of glass powder, 32 parts of silicon powder, 43 parts of filling-grade talc, 2.5 parts of borax, and 2.5 parts of solid additives. The solid additives are composed of an organosilicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 78:22.
[0052] Component B is formed by mixing 52 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 55%, 18 parts of ZnO nanoparticles, 12 parts of water, and 1.5 parts of a liquid additive. The liquid additive is composed of a film-forming additive (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 1:3.
[0053] (2) The above-mentioned component A and component B are mixed in a mass ratio of 50:50 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0054] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0055] Example 6 A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating comprises the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 38 parts of glass powder, 45 parts of silicon micropowder, 52 parts of filler-grade talc and 4 parts of solid additives, wherein the solid additives are composed of an organic silicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 60:30.
[0056] Component B is formed by mixing 68 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 40%, 25 parts of PVA@Ti-DMF of this embodiment, 16 parts of water, and 3 parts of a liquid additive, wherein the liquid additive is composed of a film-forming aid (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 0.5:2.
[0057] (2) The above-mentioned component A and component B are mixed in a mass ratio of 30:60 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0058] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0059] Example 7 1. A method for preparing an ultraviolet absorber, comprising the following steps: mixing a 5% polyvinyl alcohol (PVA) aqueous solution and SnO2 nanoparticles at a mass ratio of 30:70, and then magnetically stirring at a speed of 600r / min for 25min. After completion, the obtained mixture is placed in a high-temperature and high-pressure reactor, the reactor temperature is set to 240°C, the pressure is set to 0.35MPa, the reaction time is set to 45min, and after completion, the solid product is filtered out to obtain an ultraviolet absorber.
[0060] 2. A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating, comprising the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 16 parts of glass powder, 25 parts of silicon micropowder, 35 parts of filling-grade talc, 2 parts of boric acid, and 1 part of solid additive. The solid additive is composed of a polyether polymer defoamer and a polycarboxylic acid water reducer in a mass ratio of 80:15.
[0061] Component B is formed by mixing 48 parts of acrylate (PA) emulsion with a solid content of 60%, 13 parts of PVA@Sn-DMF of this embodiment, 8 parts of water, and 1 part of a liquid additive, wherein the liquid additive is composed of a film-forming aid (phenoxypropanol) and a dispersant (sodium hexametaphosphate) in a mass ratio of 2:5.
[0062] (2) The above-mentioned component A and component B are mixed in a mass ratio of 60:30 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0063] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0064] Example 8 1. A method for preparing an ultraviolet absorber, comprising the following steps: (1) TiO2 nanoparticles and N,N-dimethylformamide (DMF) were mixed in a mass ratio of 20:75, heated in a water bath to 95°C, and stirred at a rate of 400 r / min for 150 min. After completion, the solid product was filtered out to obtain the active precursor (Ti-DMF) for later use.
[0065] (2) Deionized water and the active precursor are mixed in a mass ratio of 60:40, and then magnetically stirred at a speed of 600 r / min for 30 minutes. After completion, the obtained mixture is placed in a high-temperature and high-pressure reactor, the reactor temperature is set to 170°C, the pressure is set to 0.75 MPa, and the reaction time is set to 110 minutes. After completion, the solid product is filtered out to obtain a UV absorber (PVA@Ti-DMF).
[0066] 2. A method for preparing an in-situ complexing ultraviolet absorbing concrete protective coating, comprising the following steps: (1) Take the following raw materials in parts by weight: Component A is formed by mixing 38 parts of glass powder, 45 parts of silicon micropowder, 52 parts of filling-grade talc, 8 parts of borax, and 4 parts of solid additives. The solid additives are composed of an organic silicon defoamer and a polycarboxylic acid water reducer in a mass ratio of 60:30.
[0067] Component B is formed by mixing 68 parts of ethylene-vinyl acetate (VAE) emulsion with a solid content of 40%, 25 parts of PVA@Ti-DMF of this embodiment, 16 parts of water, and 3 parts of a liquid additive, wherein the liquid additive is composed of a film-forming aid (polyvinyl pyrrolidone) and a dispersant (sodium tripolyphosphate) in a mass ratio of 0.5:2.
[0068] (2) The above-mentioned component A and component B are mixed in a mass ratio of 30:60 and stirred evenly to obtain the in-situ complexed ultraviolet absorption concrete protective coating.
[0069] The various properties of the spraying material prepared in this embodiment were tested, and the results are shown in the following table. Among them: the elongation at break was measured according to the standard of GB / T 23445-2009, the bonding strength was measured according to the standard of GB / T 23445-2009, the anti-seepage pressure was measured according to the standard of JC / T 2090-2011, and the tensile strength retention rate after ultraviolet treatment was measured according to the standard of GB / T 23445-2009: .
[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A UV absorber, the structural formula of which is shown below: ; In the above formula, M includes at least one of the metal elements Zn, Ti, and Sn.
2. An in-situ complexing UV absorbing concrete protective coating, characterized in that: The coating includes an in-situ complexed UV absorber as shown in the following formula: ; In the above formula, M includes at least one of the metal elements Zn, Ti, and Sn.
3. An in-situ complexing UV absorbing concrete protective coating, characterized in that: The coating comprises the following raw materials in parts by weight: Component A includes 16-38 parts of glass powder, 25-45 parts of silicon powder, 35-52 parts of talc, 2-8 parts of borate ion source, and 1-4 parts of solid additive; Component B comprises 48-68 parts of polymer emulsion, 13-25 parts of ultraviolet absorber, 8-16 parts of water, and 1-3 parts of liquid additive; wherein: the ultraviolet absorber is as described in claim 1.
4. The in-situ complexing ultraviolet absorption concrete protective coating according to claim 3, characterized in that: The mass ratio of the A component to the B component is 30-60:30-60.
5. The in-situ complexed UV absorbing concrete protective coating according to claim 3, characterized in that: The borate ion source includes at least one of borax and boric acid; Optionally, the solid additive includes at least one of a defoamer and a water reducing agent; Optionally, the mass ratio of the defoamer to the water reducing agent is 60-80:15-30; Optionally, the defoamer includes at least one of a polyether polymer defoamer and a silicone defoamer; Optionally, the water reducer includes at least one of a polycarboxylate water reducer and a naphthalene-based water reducer.
6. The in-situ complexed UV absorbing concrete protective coating according to claim 3, characterized in that: The liquid additive includes at least one of a film-forming additive and a dispersant; Optionally, the mass ratio of the film-forming aid to the dispersant is 0.5~2:2~5; Optionally, the film-forming aid includes at least one of polyvinyl pyrrolidone, phenoxypropanol; Optionally, the dispersant includes at least one of sodium tripolyphosphate and sodium hexametaphosphate; Optionally, the polymer emulsion includes at least one of ethylene-vinyl acetate emulsion and acrylate emulsion; Optionally, the solid content of the polymer emulsion is in the range of 40% to 60%.
7. The in-situ complexing ultraviolet absorption concrete protective coating according to any one of claims 3 to 6, characterized in that: The preparation method of the ultraviolet absorber comprises the following steps: (1) mixing metal oxide nanoparticles and N,N-dimethylformamide and heating them for reaction, and separating the solid product after completion to obtain the active precursor for later use; (2) Mixing the polyvinyl alcohol aqueous solution and the active precursor and subjecting them to a hydrothermal reaction; after the reaction is completed, separating out a solid product to obtain a UV absorber.
8. The in-situ complexed UV absorbing concrete protective coating according to claim 7, characterized in that: In step (1), the mass ratio of the metal oxide nanoparticles to N,N-dimethylformamide is 20-40:55-75; Optionally, in step (1), the heating temperature is 95-145° C., the reaction time is 90-150 min, the shear rate is 400-800 r / min, and preferably, continuous stirring is performed during the reaction.
9. The in-situ complexed UV absorbing concrete protective coating according to claim 7, characterized in that: In step (2), the mass fraction of the polyvinyl alcohol aqueous solution is 2-5%; Optionally, in step (2), the mass ratio of the polyvinyl alcohol aqueous solution to the active precursor is 30-60:40-70; Optionally, in step (2), the temperature of the hydrothermal reaction is 170-240° C., the pressure is 0.35-0.75 MPa, and the time is 45 min-110 min.
10. The method for preparing the in-situ complexing ultraviolet absorption concrete protective coating according to any one of claims 3 to 9, characterized in that: The method comprises the following steps: uniformly mixing the component A and the component B to obtain the coating.
Citation Information
Patent Citations
Polyvinyl alcohol-zinc oxide composite microspheres as well as preparation method and application thereof
CN108529754A
Preparation method of PVC (polyvinyl chloride) hydrophilic functional aid
CN115246973A
Organic-inorganic composite ultraviolet absorbent with excellent ultraviolet resistance as well as preparation method and application of organic-inorganic composite ultraviolet absorbent
CN118185125A
Cited By
Nanometer metal gel admixture as well as preparation method and application thereof
CN119505049A
Long-acting anti-ultraviolet aging water-based multicolor paint and preparation method thereof
CN119875439A