Multi-block polycarboxylic acid dispersing agent as well as preparation method and application thereof
Multi-block polycarboxylic acid dispersants are synthesized in aqueous solution through RAFT polymerization technology, which solves the problems of uncontrollable structure and uneven molecular weight distribution of polycarboxylic acid dispersants in coal-water slurry technology, and achieves better coal dispersion stability. and fluidity, improving the quality and combustion efficiency of coal-water slurry and reducing pollution emissions.
Patent Information
- Application Number
- CN202410754923.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing polycarboxylic acid dispersants in coal-water slurry technology have problems such as uncontrollable structure, uneven molecular weight distribution, poor viscosity reduction effect and poor slurry stability, which affects its application effect and reliability.
Reversible addition-fragmentation chain transfer (RAFT) polymerization technology is used to synthesize multi-block polycarboxylic acid dispersants in aqueous solution. By precisely controlling the monomer ratio and polymerization reaction conditions, a hydrophobic long carbon chain and hydrophilic short side chain are designed. Structured block copolymer to improve dispersion and stability.
It achieves precise control of the molecular weight and molecular weight distribution of the dispersant, significantly improves the dispersion stability and fluidity of coal, reduces agglomeration between coal particles, improves product quality and combustion efficiency, and reduces pollution emissions.
Smart Images

Figure CN118725215A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer synthesis and coal-water slurry, and specifically relates to a multi-block polycarboxylic acid dispersant and a preparation method and application thereof. Background Art
[0002] In current industrial applications, especially in the field of water-coal slurry technology, the use of dispersants is crucial to improving the dispersion of coal in water and reducing the overall viscosity of the system. With the increasing environmental protection requirements and the pursuit of efficient energy utilization, the development of new dispersants with efficient dispersibility and environmentally friendly properties has become an important demand of the industry. Traditional polycarboxylic acid dispersants are prepared by random copolymerization. Although this method is simple, it often encounters problems such as unclear molecular structure, difficulty in molecular weight control, and large polymerization distribution index (PDI), resulting in large differences in dispersant performance between different batches, which seriously affects its application effect and reliability in fields such as water-coal slurry.
[0003] In recent years, reversible addition-fragmentation chain transfer (RAFT) polymerization technology has attracted widespread attention in the field of polymer science due to its excellent molecular weight control ability and designability. RAFT polymerization technology can accurately control the structure of polymers at the molecular level, including molecular weight and molecular weight distribution, thereby significantly improving the performance stability of the final product. In addition, RAFT polymerization technology is not only applicable to polymerization reactions in organic solvents, but can also be carried out in aqueous solutions, providing a new approach for the development of environmentally friendly high-performance polymers. Despite this, there is relatively little research on the application of RAFT technology in aqueous solutions, especially in the preparation of multi-block polycarboxylic acid dispersants, and its potential in practical applications such as water-coal slurries has not yet been fully explored. Summary of the invention
[0004] The object of the present invention is to provide a multi-block polycarboxylic acid dispersant and a preparation method and application thereof, which solve the problems of uncontrollable structure, uneven molecular weight distribution, poor viscosity reduction effect and slurry stability of existing dispersants.
[0005] The present invention is achieved through the following technical solutions:
[0006] A multi-block polycarboxylic acid dispersant, the structural formula of which is as follows:
[0007]
[0008] in,
[0009] n is selected from an integer of 5-25; n1 is selected from an integer of 5-20; n2 is selected from an integer of 20-40; n3 is selected from an integer of 10-30.
[0010] Furthermore, the raw materials include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent;
[0011] The molar ratio of monomer I, monomer II and monomer III is (0.1-2):4:1.
[0012] Further, the monomer I is one or more of allyl polyoxyethylene ether 200, allyl polyoxyethylene ether 400, allyl polyoxyethylene ether 600 and allyl polyoxyethylene ether 1200;
[0013] The monomer II is one or more of acrylic acid, methacrylic acid, methacrylate and sodium methacrylate;
[0014] The monomer III is one or more of sodium p-styrene sulfonate, sodium methyl propylene sulfonate, and sodium 2-acrylamido-2-methylpropane sulfonate;
[0015] The initiator is one or more of azobisisobutylamidine hydrochloride, dimethyl azobisisobutyrate and dibenzoyl peroxide;
[0016] The chain transfer agent is one or more of dithiocarbamate, xanthate and trithiocarbonate.
[0017] Furthermore, the number average molecular weight of the multi-block polycarboxylic acid dispersant is in the range of 9000 to 97000, and the PDI is controlled in the range of 1.30 to 2.60.
[0018] The present invention also discloses a method for preparing a multi-block polycarboxylic acid dispersant, comprising the following steps:
[0019] S1, mixing and stirring the monomer I containing an allyl structure and deionized water to prepare an initial mixed solution;
[0020] Add initiator and chain transfer agent to the initial mixed solution and continue stirring until completely dissolved;
[0021] The polymerization reaction was carried out under a nitrogen atmosphere, and after the polymerization was completed, preliminary purification was performed to obtain product Ⅰ;
[0022] S2, mixing the product I with deionized water to obtain a product I solution, and heating the product I solution;
[0023] The initiator and the monomer II containing a carboxylic acid functional group are dissolved in deionized water to obtain two solutions;
[0024] Under a continuous nitrogen protective atmosphere, these two solutions were gradually added to the product I solution for polymerization reaction to obtain a more purified solution;
[0025] The pH of the more purified solution was adjusted to neutral using an alkaline solution, followed by further purification to obtain product II;
[0026] S3, mixing the product II with deionized water to obtain a product II solution;
[0027] The initiator and the monomer III containing the sulfonate functional group are dissolved in the product II solution, and a polymerization reaction is carried out under a nitrogen protective atmosphere. After the polymerization is completed, the multi-block polycarboxylic acid dispersant is obtained by dialysis and freeze drying.
[0028] Further, in S1, the chain transfer agent is 0.5% to 2.5% by mass of the monomer I;
[0029] The initiator is 0.1%-2.0% by mass of monomer I.
[0030] Further, in S2, the mass ratio of monomer II to product I is 0.2-0.5:1;
[0031] The initiator is 0.1%-2.0% of the mass of monomer II.
[0032] Further, in S3, the mass ratio of monomer III to product II is 0.15-0.4:1;
[0033] The initiator is 0.1%-2.0% of the mass of monomer III.
[0034] Furthermore, the polymerization reaction temperature is 70-80° C., and the reaction time is 4-8 hours.
[0035] The invention also discloses the application of the multi-block polycarboxylic acid dispersant in the field of preparing water-coal slurry.
[0036] Compared with the prior art, the present invention has the following beneficial technical effects:
[0037] The present invention discloses a multi-block polycarboxylic acid dispersant, which is composed of a hydrophobic long carbon chain and a short side chain providing steric hindrance and wetting properties. Allyl polyoxyethylene ether is selected as a macromonomer, and carboxyl functional monomers and sulfonic acid functional monomers providing hydrophilic groups are side chain structures. The long carbon chain is a hydrophobic structure for contacting the surface of low-rank coal; the allyl polyoxyethylene ether and R1 containing a carboxylic acid functional group are a hydrophilic structure for contacting water. Through molecular structure design, compared with polymers prepared by traditional free radical polymerization, the block copolymer prepared by the present invention has better dispersibility and slurry stability as a water-coal slurry dispersant. The hydrophilic group (-SO3 -) chelates with the mineral surface through electrostatic repulsion, while the benzene ring interacts with the aromatic ring on the coal surface, thereby improving the stability of the dispersant. In addition, the long side chain of the dispersant forms a large hydration film with water, while the short chain (-SO3 - ) and (-COO - ) provides electrostatic repulsion, making the coal particles evenly dispersed. In this way, the dispersant not only enhances the dispersion stability of coal, but also improves its fluidity. The addition of dispersants changes the content of elements such as C and O on the surface of coal. Dispersants increase the oxygen-containing functional groups on the surface of coal, and dispersants can effectively reduce the agglomeration phenomenon between coal particles. Thereby improving product quality, combustion efficiency, and reducing pollution emissions.
[0038] The present invention also discloses a method for preparing a multi-block polycarboxylic acid dispersant. The present invention adopts a reversible addition-fragmentation transfer method (RAFT) to synthesize a multi-block polycarboxylic acid dispersant in an aqueous solution. Compared with traditional free radical polymerization, its structure and molecular weight are controllable and the molecular weight distribution is uniform; RAFT polymerization can regulate the reaction rate, design the molecular weight of the polymer and obtain a lower PDI. By adjusting the reaction conditions, the molecular weight and molecular weight distribution of the polymer can be accurately controlled, thereby preparing a block polycarboxylic acid dispersant with excellent performance.
[0039] In S1, monomer I containing an allyl structure, an initiator and a chain transfer agent are polymerized to form a main chain of polycarboxylic acid from carbon-carbon double bonds, which can be adsorbed on the hydrophobic part of the coal surface, and the molecules of the dispersant are adsorbed on the surface of coal particles through interaction forces such as van der Waals forces. Long side chain allyl polyoxyethylene ether is added, connected to the main chain through a double bond, one end is connected to the main chain of the dispersant, and the other end extends into the water to form a hydrogen bond with water and provide a steric hindrance effect.
[0040] In S2, a functional side chain containing a carboxyl group is added, and monomer II is added. The short side chain structure is a carboxyl functional monomer that provides a hydrophilic group and is connected to the main chain through a CC bond. - It comes in contact with water and provides electrostatic repulsion, and can be combined with a variety of monomers to work synergistically.
[0041] In S3, a sulfonic acid functional side chain is added, monomer III is added, and a sulfonic acid functional monomer providing a hydrophilic group is introduced to connect the main chain through a CC bond. - The hydrophilic groups provide electrostatic repulsion and adsorb on the mineral surface through chelation. The benzene ring can interact with the aromatic ring on the surface of coal to enhance stability. - and -SO3 - When the hydrophilic groups are diverse, they will affect the performance of anionic dispersants. - The adsorption affinity is stronger than that of -SO3- , because -COO - The chelating ability is better than -SO3 - . -COO - Can be used as an anchoring group, while -SO3 - The groups are oriented toward the water phase.
[0042] The slurry viscosity test of low-rank coal using block copolymer and random copolymer dispersants showed that under the conditions of slurry concentration of 64.0% and dispersant addition of 0.4%, the block polycarboxylic acid dispersant has lower viscosity and better stability than the slurry prepared using random polycarboxylic acid dispersant due to its structural advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The synthetic route of the multi-block polycarboxylic acid dispersant in the present invention;
[0044] Figure 2 It is the infrared spectrum of the multi-block polycarboxylic acid dispersant in the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments.
[0046] The components described and shown in the drawings and embodiments of the present invention may be arranged and designed in various configurations. Therefore, the detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of the claimed invention, but merely represents a selected embodiment of the present invention. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0047] It should be noted that the terms "comprises", "includes" or any other variations are intended to cover non-exclusive inclusion, so that a process, element, method, article or equipment that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to the process, element, method, article or equipment.
[0048] The features and performances of the present invention are further described in detail below in conjunction with the embodiments.
[0049] These examples show how to adjust the experimental conditions or materials based on the original experimental steps to obtain products with different properties. Using APEG, AA and SSS as monomers, two polycarboxylic acid dispersants PC with different structures were synthesized by random copolymerization and RAFT method. r and PC b。 Note that the following content is a schematic description and needs to be adjusted according to experimental results and product requirements in actual applications.
[0050] Example 1: (the molar ratio of monomer I, monomer II and monomer III is 0.5:4:1):
[0051] The raw materials of the multi-block polycarboxylic acid dispersant prepared in this embodiment include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; monomer I is allyl polyoxyethylene ether 600 (APEG600), monomer II is acrylic acid AA, monomer III is sodium p-styrene sulfonate (SSS), the initiator is azobisisobutylamidine hydrochloride (AIBA), and the chain transfer agent is S, S'di(α, α'methyl α"acetic acid)-trithiocarbonate TRIT.
[0052] The molar ratio of allyl polyoxyethylene ether 600 (APEG600), acrylic acid AA and sodium p-styrene sulfonate (SSS) is 0.5:4:1.
[0053] Step 1: In a 250 mL three-necked flask equipped with a stirrer and a condenser, add 7.5 g APEG600 and 15 g water to form an initial mixed solution.
[0054] Subsequently, 0.0375 g of AIBA and 0.117 g of TRIT, a transfer agent, were added to the initial mixed solution and stirred to fully dissolve. The temperature was raised to 70°C and nitrogen was introduced to isolate the air for 30 minutes. The reaction was continued at 70°C for 8 hours. After the reaction was completed, the mixture was dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 3000. The dialyzed product was freeze-dried to obtain product I.
[0055] Step 2: Add product I into a new 250 mL three-necked flask, raise the temperature to 70 °C again and continue stirring;
[0056] Dissolve 0.036g AIBA in 15g water and 7.2g AA in 7.8g deionized water. Under the condition of continuous nitrogen flow, AIBA solution and AA solution were evenly added to the three-necked flask by a peristaltic pump, and the addition time was set to 30 minutes. After the addition was completed, the reaction was continued at 70°C for 8 hours. After the reaction was completed, the pH was adjusted to about 7 with 30% NaOH solution. The product was dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 5000. After dialysis, a relatively pure dialysis product was obtained by freeze drying as product II.
[0057] If AIBA is added directly, a large number of free radicals will be generated during the heating reaction, making the polymerization reaction uncontrollable, so it must be dissolved and added dropwise to control the free radical initiation rate.
[0058] Step 3: Weigh 6 g of the product II obtained in step 2 and 17.45 g of water into a 150 mL three-necked flask and heat to 70°C while stirring.
[0059] 0.01137 g of AIBA and 2.575 g of SSS were weighed and dissolved in deionized water. The solution of AIBA and SSS was added to a flask under nitrogen protection. After 8 hours of reaction, dialysis was performed for 24 hours using a dialysis bag with a molecular weight cutoff of 8000. After dialysis, the tri-monomer block polycarboxylic acid dispersant PCb1 was obtained by freeze drying.
[0060] like Figure 1 As shown, this reaction can be divided into three stages:
[0061] The first stage: Under the action of the chain transfer agent, the carbon-sulfur bond is broken, and monomer I is reversibly added to the broken carbon-sulfur bond to obtain product I.
[0062] The second stage: The carbon-carbon bond with carboxyl group in monomer II is broken and reversibly added to the carbon-sulfur bond of product I to form product II.
[0063] The third stage: the carbon-carbon double bond with the benzenesulfonic acid group is reversibly added to the carbon-sulfur bond of product II to generate product III, which is a monomer block polycarboxylic acid dispersant.
[0064] Example 2: (the molar ratio of monomer I, monomer II and monomer III is 0.75:4:1):
[0065] The raw materials of the multi-block polycarboxylic acid dispersant prepared in this embodiment include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; monomer I is allyl polyoxyethylene ether 600 (APEG600), monomer II is methacrylic acid (MA), monomer III is sodium methyl methacrylate sulfonate (SMAS), the initiator is dimethyl azobisisobutyrate, and the chain transfer agent is S, S'di(α, α'methyl α"acetic acid)-trithiocarbonate TRIT.
[0066] The molar ratio of allyl polyoxyethylene ether 600 (APEG600), methacrylic acid (MA) and sodium p-methylacrylic acid sulfonate (SMAS) is 0.75:4:1.
[0067] Step 1: In a 250mL three-necked flask equipped with a stirrer and a condenser, add 11.22g APEG600 and 20.2g water to form an initial mixed solution. Subsequently, 0.0561g dimethyl azobisisobutyrate and 0.175g TRIT, a transfer agent, were added to the mixed solution and stirred to fully dissolve. The temperature was raised to 70°C and nitrogen was introduced to isolate the air for 30 minutes. The reaction was continued at 70°C for 8 hours. After the reaction was completed, dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 3000. The dialyzed product was freeze-dried to obtain product I.
[0068] Step 2: Add product I to a new 250mL three-necked flask. Raise the temperature to 70°C again and continue stirring. Dissolve 0.036g of dimethyl azobisisobutyrate in 15g of water and 7.2g of methacrylic acid in 7.8g of deionized water. Under the condition of continuous nitrogen flow, dimethyl azobisisobutyrate and methacrylic acid solution are evenly added to the three-necked flask by a peristaltic pump, and the addition time is set to 30 minutes. After the addition is completed, the reaction is continued at 70°C for 8 hours. After the reaction is completed, the pH is adjusted to about 7 with 30% NaOH solution. The product is dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 5000. After dialysis, a relatively pure dialyzed product is obtained by freeze drying as product II.
[0069] Step 3: Weigh 7g of product II obtained in step 2 and 22.34g of water into a 150mL three-necked flask. Heat to 70°C while stirring. According to the molar ratio of step 1 and step 2, weigh 0.01137g of dimethyl azobisisobutyrate and 2.575g of sodium methyl propylene sulfonate, and dissolve them in deionized water. Add the solution of dimethyl azobisisobutyrate and sodium methyl propylene sulfonate to the flask under nitrogen protection. After 8 hours of reaction, use a dialysis bag with a molecular weight cutoff of 8000 for 24 hours of dialysis. After dialysis, the three-monomer block polycarboxylic acid dispersant PCb2 was obtained by freeze drying.
[0070] Example 3: (the molar ratio of monomer I, monomer II and monomer III is 1:4:1):
[0071] The raw materials of the multi-block polycarboxylic acid dispersant prepared in this embodiment include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; monomer I is allyl polyoxyethylene ether 600 (APEG600), monomer II is methyl acrylate, monomer III is sodium 2-acrylamido-2-methylpropane sulfonate, the initiator is dibenzoyl peroxide, and the chain transfer agent is S, S' di(α, α' methyl α" acetic acid)-trithiocarbonate TRIT.
[0072] The molar ratio of allyl polyoxyethylene ether 600 (APEG600), methacrylate and sodium 2-acrylamido-2-methylpropane sulfonate is 1:4:1.
[0073] Step 1: In a 250mL three-necked flask equipped with an agitator and a condenser, add 15g APEG600 and 29.50g water to form an initial mixed solution. Subsequently, add 0.075g dibenzoyl peroxide and 0.234g TRIT, a transfer agent, to the mixed solution and stir to fully dissolve it. Raise the temperature to 70°C and introduce nitrogen to isolate the air for 30 minutes. Continue the reaction at 70°C for 8 hours. After the reaction is completed, dialyze for 24 hours using a dialysis bag with a molecular weight cutoff of 3000. The dialyzed product is freeze-dried.
[0074] Step 2: Weigh the same amount of dialyzed product as in step 1 and add it to a new 250mL three-necked flask. Raise the temperature to 70°C again and continue stirring. Dissolve 0.036g of dibenzoyl peroxide in 15g of water and 7.2g of methacrylate in 7.8g of deionized water. Under the condition of continuous nitrogen flow, dibenzoyl peroxide and methacrylate solution are evenly added to the three-necked flask by a peristaltic pump, and the addition time is set to 30 minutes. After the addition is completed, the reaction is continued at 70°C for 8 hours. After the reaction is completed, the pH is adjusted to about 7 with 30% NaOH solution. The product is dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 5000. After dialysis, a relatively pure dialyzed product is obtained by freeze drying.
[0075] Step 3: Weigh 8g of the dialyzed product obtained in step 2 and 25.67g of water into a 150mL three-necked flask. Heat to 70°C while stirring. According to the molar ratio of step 1 and step 2, weigh 0.01137g of methacrylate and 2.575g of sodium 2-acrylamide-2-methylpropane sulfonate and dissolve them in deionized water. Add the solution of methacrylate and methacrylate to the flask under nitrogen protection. After 8 hours of reaction, use a dialysis bag with a molecular weight cutoff of 8000 for 24 hours of dialysis. After dialysis, the three-monomer block polycarboxylic acid dispersant PCb3 was obtained by freeze drying.
[0076] Example 4: (the molar ratio of monomer I, monomer II and monomer III is 1.25:4:1):
[0077] The raw materials of the multi-block polycarboxylic acid dispersant prepared in this embodiment include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; monomer I is allyl polyoxyethylene ether 600 (APEG600), monomer II is acrylic acid AA, monomer III is sodium p-styrene sulfonate (SSS), the initiator is azobisisobutylamidine hydrochloride (AIBA), and the chain transfer agent is S, S'di(α, α'methyl α"acetic acid)-trithiocarbonate TRIT.
[0078] The molar ratio of allyl polyoxyethylene ether 600 (APEG600), acrylic acid AA and sodium p-styrene sulfonate (SSS) is 1.25:4:1.
[0079] Step 1: In a 250mL three-necked flask equipped with an agitator and a condenser, add 18.75g APEG600 and 37.75g water to form an initial mixed solution. Subsequently, add 0.0937g AIBA and 0.292g TRIT, a transfer agent, to the mixed solution and stir to fully dissolve it. Raise the temperature to 70°C and introduce nitrogen to isolate the air for 30 minutes. Continue the reaction at 70°C for 8 hours. After the reaction is completed, dialyze for 24 hours using a dialysis bag with a molecular weight cutoff of 3000. The dialyzed product is freeze-dried.
[0080] Step 2: Weigh the same amount of dialyzed product as in step 1 and add it to a new 250mL three-necked flask. Raise the temperature to 70°C again and continue stirring. Dissolve 0.036gAIBA in 15g water and 7.2gAA in 7.8g deionized water. Under the condition of continuous nitrogen flow, AIBA and AA solutions are evenly added to the three-necked flask by a peristaltic pump, and the addition time is set to 30 minutes. After the addition is completed, continue the reaction at 70°C for 8 hours. After the reaction is completed, adjust the pH to about 7 with 30% NaOH solution. Use a dialysis bag with a molecular weight cutoff of 5000 to dialyze the product for 24 hours. After dialysis, a relatively pure dialysis product is obtained by freeze drying.
[0081] Step 3: Weigh 9 g of the dialyzed product obtained in step 2 and 27 g of water and add them to a 150 mL three-necked flask. Heat to 70°C while stirring. Weigh 0.01137 g of AIBA and 2.575 g of SSS according to the molar ratio of step 1 and step 2, and dissolve them in deionized water. Add the solution of AIBA and SSS to the flask under nitrogen protection. After 8 hours of reaction, use a dialysis bag with a molecular weight cutoff of 8000 for 24 hours of dialysis. After dialysis, the three-monomer block polycarboxylic acid dispersant PCb4 was obtained by freeze drying.
[0082] Example 5: (the molar ratio of monomer I, monomer II and monomer III is 1.5:4:1):
[0083] The raw materials of the multi-block polycarboxylic acid dispersant prepared in this embodiment include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; monomer I is allyl polyoxyethylene ether 1200 (APEG1200), monomer II is acrylic acid AA, monomer III is sodium p-styrene sulfonate (SSS), the initiator is azobisisobutylamidine hydrochloride (AIBA), and the chain transfer agent is S, S'di(α, α'methyl α"acetic acid)-trithiocarbonate TRIT.
[0084] The molar ratio of allyl polyoxyethylene ether 1200 (APEG1200), acrylic acid AA and sodium p-styrene sulfonate (SSS) is 1.5:4:1.
[0085] Step 1: In a 250mL three-necked flask equipped with an agitator and a condenser, 22.44g APEG1200 and 46.36g water were calculated and added according to the molar ratio of AA, APEG1200 and SSS of 4:1.5:1 to form an initial mixed solution. Subsequently, 0.1122g AIBA and 0.35g TRIT, a transfer agent, were added to the mixed solution and stirred to fully dissolve. The temperature was raised to 70°C and nitrogen was introduced to isolate the air for 30 minutes. The reaction was continued at 70°C for 8 hours. After the reaction was completed, dialyzed for 24 hours using a dialysis bag with a molecular weight cutoff of 3000. The dialyzed product was freeze-dried.
[0086] Step 2: Weigh the same amount of dialyzed product as in step 1 and add it to a new 250mL three-necked flask. Raise the temperature to 70°C again and continue stirring. Dissolve 0.036g AIBA in 15g water and 7.2g AA in 7.8g deionized water. Under the condition of continuous nitrogen flow, AIBA and AA solutions are evenly added to the three-necked flask by a peristaltic pump, and the addition time is set to 30 minutes. After the addition is completed, continue the reaction at 70°C for 8 hours. After the reaction is completed, adjust the pH to about 7 with 30% NaOH solution. Use a dialysis bag with a molecular weight cutoff of 5000 to dialyze the product for 24 hours. After dialysis, a relatively pure dialysis product is obtained by freeze drying.
[0087] Step 3: Weigh 12g of the dialyzed product obtained in step 2 and 30.10g of water into a 150mL three-necked flask. Heat to 70°C while stirring. Weigh 0.01137g of AIBA and 2.575g of SSS according to the molar ratio of step 1 and step 2, and dissolve them in deionized water. Add the solution of AIBA and SSS to the flask under nitrogen protection. After 8 hours of reaction, use a dialysis bag with a molecular weight cutoff of 8000 for 24 hours of dialysis. After dialysis, the tri-monomer block polycarboxylic acid dispersant PCb5 was obtained by freeze drying.
[0088] Specifically, monomer I is one or more of allyl polyoxyethylene ether 200, allyl polyoxyethylene ether 400, allyl polyoxyethylene ether 600 and allyl polyoxyethylene ether 1200;
[0089] The monomer II is one or more of acrylic acid, methacrylic acid, methacrylate and sodium methacrylate;
[0090] The monomer III is one or more of sodium p-styrene sulfonate, methyl styrene, styrene, and sodium 2-acrylamido-2-methylpropane sulfonate;
[0091] The initiator is one or more of azobisisobutylamidine hydrochloride, dimethyl azobisisobutyrate and dibenzoyl peroxide;
[0092] The chain transfer agent is one or more of dithiocarbamate, xanthate and trithiocarbonate.
[0093] The materials are not limited to the 5 embodiments, and the principles are the same and will not be described in detail.
[0094] Comparative Example 1: (molar ratio: 0.5:4:1):
[0095] A 250 mL three-necked flask was loaded with a magnetic stirrer and a condenser. According to the molar ratio of APEG600:AA:SSS = 0.5:4:1, 7.2 g of acrylic acid (AA), 7.5 g of allyl polyoxyethylene ether (APEG600) and 2.575 g of sodium p-styrene sulfonate (SSS) were added to the flask, and an appropriate amount of deionized water was added. Weigh 0.4% potassium persulfate (KPS) of the total mass of the monomer as an initiator and dissolve it in deionized water. Stir and heat to 70°C and pass nitrogen. KPS and AA solutions were dripped into the flask through a peristaltic pump for 1 hour. After maintaining the reaction at 70°C for 6 hours, cool it and adjust the pH to 7 with 30% NaOH solution. Obtain the random block polycarboxylic acid dispersant PCr1.
[0096] Comparative Example 2: (molar ratio: 0.75:4:1):
[0097] A 250 mL three-necked flask was loaded with a magnetic stirrer and a condenser. According to the molar ratio of APEG600:MA:SMAS = 0.75:4:1, 7.2 g of methacrylic acid (MA), 11.22 g of allyl polyoxyethylene ether (APEG600) and 2.575 g of sodium methyl propylene sulfonate (SMAS) were added to the flask, and an appropriate amount of deionized water was added. Weigh 0.4% potassium persulfate (KPS) of the total mass of the monomer as an initiator and dissolve it in deionized water. Stir and heat to 70°C and pass nitrogen. KPS and MA solutions were dripped into the flask by a peristaltic pump for 1 hour. After maintaining the reaction at 70°C for 6 hours, cool it and adjust the pH to 7 with 30% NaOH solution. Obtain the random block polycarboxylic acid dispersant PCr2.
[0098] Comparative Example 3: (molar ratio: 1:4:1):
[0099] A 250 mL three-necked flask was loaded with a magnetic stirrer and a condenser. According to the molar ratio of APEG600: methacrylate: 2-acrylamide-2-methylpropanesulfonate = 1:4:1, 7.2 g methacrylate, 15 g allyl polyoxyethylene ether (APEG600) and 2.575 g 2-acrylamide-2-methylpropanesulfonate were added to the flask, and an appropriate amount of deionized water was added. Weigh 0.4% potassium persulfate (KPS) of the total mass of the monomer as an initiator and dissolve it in deionized water. Stir and heat to 70 ° C and pass nitrogen. KPS and methacrylate solution were dripped into the flask by a peristaltic pump for 1 hour. After maintaining the reaction at 70 ° C for 6 hours, cool it and adjust the pH to 7 with 30% NaOH solution. Obtain the random block polycarboxylic acid dispersant PCr3.
[0100] Comparative Example 4: (molar ratio: 1.25:4:1):
[0101] A 250 mL three-necked flask was equipped with a magnetic stirrer and a condenser. According to the molar ratio of APEG600:AA:SSS = 1.25:4:1, 7.2 g of acrylic acid (AA), 18.75 g of allyl polyoxyethylene ether (APEG600) and 2.575 g of sodium p-styrene sulfonate (SSS) were added to the flask, and an appropriate amount of deionized water was added. Weigh 0.4% potassium persulfate (KPS) of the total mass of the monomer as an initiator and dissolve it in deionized water. Stir and heat to 70°C and pass nitrogen. KPS and AA solutions were dripped into the flask by a peristaltic pump for 1 hour. After maintaining the reaction at 70°C for 6 hours, cool it and adjust the pH to 7 with 30% NaOH solution. Obtain the random block polycarboxylic acid dispersant PCr4.
[0102] Comparative Example 5: (molar ratio: 1.5:4:1):
[0103] A 250 mL three-necked flask was equipped with a magnetic stirrer and a condenser. According to the molar ratio of APEG1200:AA:SSS = 1.5:4:1, 7.2 g of acrylic acid (AA), 22.44 g of allyl polyoxyethylene ether (APEG1200) and 2.575 g of sodium p-styrene sulfonate (SSS) were added to the flask, and an appropriate amount of deionized water was added. Weigh 0.4% potassium persulfate (KPS) of the total mass of the monomer as an initiator and dissolve it in deionized water. Stir and heat to 70°C and pass nitrogen. KPS and AA solutions were dripped into the flask by a peristaltic pump for 1 hour. After maintaining the reaction at 70°C for 6 hours, cool it and adjust the pH to 7 with 30% NaOH solution. Obtain the random block polycarboxylic acid dispersant PCr5.
[0104] Embodiment effect description:
[0105] In the present invention, the rheological properties of a specific coal water slurry formulation were evaluated by rheological testing methods. Using Hongliulin mixed coal, a 64.0% coal water slurry was prepared according to a multimodal proportioning ratio, and 0.4% dispersant was added to optimize the rheological properties. The viscosity test of the coal water slurry was carried out at a constant temperature of 25°C, and a coal water slurry viscometer was used to measure the shear rate from 0s -1 Up to 100s -1 , in 100s -1 It stabilizes for a while and then increases from 100s -1 Down to 0s -1 , the shear rate is stable at 100s -1 The average apparent viscosity of water-coal slurry at .
[0106] Table 1 Molecular weight of random and block dispersants
[0107]
[0108] It can be seen from Table 1 that with the adjustment of the monomer ratio, the relative molecular weight (M n and M w ) and molecular weight distribution (PDI) show significant differences. The molecular weight of random polycarboxylic acids is generally higher than that of block polycarboxylic acids, while the molecular weight distribution of block polycarboxylic acids is relatively narrower.
[0109] The present invention proves that by precisely controlling the polymerization conditions and monomer ratios, it is possible to precisely control the molecular weight and distribution of polycarboxylic acid dispersants. In particular, by using RAFT polymerization technology, block polycarboxylic acids with better molecular weight control and narrower molecular weight distribution can be synthesized compared to traditional random copolymerization methods, providing a new approach for the development of high-performance polycarboxylic acid dispersants.
[0110] Table 2 Comparison of viscosity of block polycarboxylic acid and random polycarboxylic acid
[0111]
[0112] It can be seen from Table 2 that, compared with random polycarboxylic acid dispersants, block polycarboxylic acid dispersants can effectively reduce the viscosity of water-coal slurry and improve its stability under the same slurrying conditions. With the increase of the proportion of macromonomer APEG, the viscosity shows a trend of first decreasing and then increasing. b 4 (nAA: nAPEG600: nSSS = 4: 1.25: 1) The minimum dispersant viscosity is 550 mPa.s. PC b 4 Dispersants show better viscosity reduction and stabilization effects on low-rank coal-water slurry (CWS). Block structured PC b4 The prepared water-coal slurry has the best slurry stability, with lower viscosity and better stability.
[0113] like Figure 2 The infrared spectra of PCb4 and PCr4 (AA:APEG 600:SSS is 4:1.25:1) are shown. APEG600, AA and SSS are the infrared spectra of three monomers of dispersant. The structure of the dispersant is analyzed at 3310 cm -1 The stretching vibration peak of carboxyl hydroxyl group is 2875cm -1 The peak at 1720 cm is the saturated methylene symmetric stretching vibration peak. -1 The -C=O stretching vibration peak is at 1630cm -1 There is no -C=C- characteristic absorption peak around 1560cm -1 There will be an absorption peak of COONa, 1400cm -1 The peak at is the bending vibration peak of methylene CH. From the above main characteristic structures, it can be judged that the infrared spectra of PCb4 and PCr4 have a high degree of overlap with the raw material spectra, indicating that the target products synthesized are consistent.
[0114] The present invention demonstrates the remarkable performance of block polycarboxylic acid dispersants in reducing the viscosity of low-rank coal-water slurries and enhancing their stability, and also provides a new technical approach for the efficient preparation of low-rank coal-water slurries, demonstrating the great potential of this type of dispersant in future practical applications.
[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A multi-block polycarboxylic acid dispersant, characterized in that: Its structural formula is as follows: R1=-COOH,-COONa-COOCH3-CONH2 R3=H or CH3 Wherein, R4=H or CH3; n is selected from an integer of 5-25; n1 is selected from an integer of 5-20; n2 is selected from an integer of 20-40; n3 is selected from an integer of 10-30.
2. The polyblock polycarboxylic acid dispersant according to claim 1, characterized in that: The raw materials include the following components: monomer I containing an allyl structure, monomer II containing a carboxylic acid functional group, monomer III containing a sulfonate functional group, an initiator and a chain transfer agent; The molar ratio of monomer I, monomer II and monomer III is (0.1-2):4:
1.
3. A multi-block polycarboxylic acid dispersant according to claim 2, characterized in that: The monomer I is one or more of allyl polyoxyethylene ether 200, allyl polyoxyethylene ether 400, allyl polyoxyethylene ether 600 and allyl polyoxyethylene ether 1200; The monomer II is one or more of acrylic acid, methacrylic acid, methacrylate and sodium methacrylate; The monomer III is one or more of sodium p-styrene sulfonate, sodium methyl propylene sulfonate, and sodium 2-acrylamido-2-methylpropane sulfonate; The initiator is one or more of azobisisobutylamidine hydrochloride, dimethyl azobisisobutyrate and dibenzoyl peroxide; The chain transfer agent is one or more of dithiocarbamate, xanthate and trithiocarbonate.
4. A multi-block polycarboxylic acid dispersant according to claim 1, characterized in that: The number average molecular weight of the multi-block polycarboxylic acid dispersant is in the range of 9000-97000, and the PDI is controlled in the range of 1.30-2.
60.
5. A method for preparing a multi-block polycarboxylic acid dispersant, characterized in that: The following steps are involved: S1, mixing and stirring the monomer I containing an allyl structure and deionized water to prepare an initial mixed solution; Add initiator and chain transfer agent to the initial mixed solution and continue stirring until completely dissolved; The polymerization reaction was carried out under a nitrogen atmosphere, and after the polymerization was completed, preliminary purification was performed to obtain product Ⅰ; S2, mixing the product I with deionized water to obtain a product I solution, and heating the product I solution; The initiator and the monomer II containing a carboxylic acid functional group are dissolved in deionized water to obtain two solutions; Under a continuous nitrogen protective atmosphere, these two solutions were gradually added to the product I solution for polymerization reaction to obtain a more purified solution; The pH of the more purified solution was adjusted to neutral using an alkaline solution, followed by further purification to obtain product II; S3, mixing product II with deionized water to obtain a product II solution; The initiator and the monomer III containing the sulfonate functional group are dissolved in the product II solution, and a polymerization reaction is carried out under a nitrogen protective atmosphere. After the polymerization is completed, the multi-block polycarboxylic acid dispersant is obtained by dialysis and freeze drying.
6. The method for preparing a multi-block polycarboxylic acid dispersant according to claim 5, characterized in that: In S1, the chain transfer agent is 0.5% to 2.5% of the mass of monomer I; The initiator is 0.1%-2.0% by mass of monomer I.
7. The method for preparing a multi-block polycarboxylic acid dispersant according to claim 5, characterized in that: In S2, the mass ratio of monomer II to product I is 0.2-0.5:1; The initiator is 0.1%-2.0% of the mass of monomer II.
8. The method for preparing a multi-block polycarboxylic acid dispersant according to claim 5, characterized in that: In S3, the mass ratio of monomer III to product II is 0.15-0.4:1; The initiator is 0.1%-2.0% of the mass of monomer III.
9. The method for preparing a multi-block polycarboxylic acid dispersant according to claim 5, characterized in that: The polymerization reaction temperature is 70-80° C., and the reaction time is 4-8 hours.
10. Use of the multi-block polycarboxylic acid dispersant according to any one of claims 1 to 4 in the field of preparing coal water slurry.
Citation Information
Patent Citations
Novel high-molecular-block dispersing agent, preparation method and application thereof
CN105418865A
Preparation method of benzene ring-containing sulfonic block modified polycarboxylic acid slump retaining agent
CN111057198A
Phenyl sulfonic block polymer modified polycarboxylate water reducer
CN111205412A
Cited By
Vanadium electrolyte multifunctional polymer additive and preparation method thereof
CN118909212A
Branched chain type polymer viscosity reducer as well as preparation method and application thereof
CN119409901A
A branched polymer viscosity reducer, its preparation method and application
CN119409901B