High-performance polypropylene composite material and preparation method thereof
By using a specific ratio of low-melt and high-melt PP resin, modified basalt fiber and modified magnesium sulfate whiskers in the polypropylene material, combined with coupling agent and zinc sulfide nanosheet treatment, the wear resistance of the polypropylene material is solved Solve the problems of insufficient elasticity and linear expansion coefficient, and achieve high performance and excellent appearance of polypropylene composite materials, which are suitable for a variety of products with high performance requirements.
Patent Information
- Application Number
- CN202410976527.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional polypropylene materials have deficiencies in wear resistance, linear expansion coefficient and surface appearance, which limit their wider application.
It uses a specific ratio of low melt mass flow rate PP resin and high melt mass flow rate PP resin, adds modified basalt fiber and modified magnesium sulfate whiskers, and is treated with a specific coupling agent and packaged with zinc sulfide nanosheets. Covering improves the wear resistance, linear expansion coefficient and mechanical properties of the material.
It achieves excellent wear resistance, low linear expansion coefficient, excellent mechanical properties and good appearance of high-performance polypropylene composite materials, and is suitable for automobiles, home appliances, electronic products and other fields.
Smart Images

Figure BDA0004954716780000091
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymer composite materials, and in particular to a high-performance polypropylene composite material and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a general-purpose plastic widely used in various fields. However, traditional polypropylene materials still need to be improved in terms of wear resistance, linear expansion coefficient and surface appearance. Although existing polypropylene composite materials have improved these properties to a certain extent, they still have problems such as insufficient wear resistance and large linear expansion coefficient, which limit their wider application. Therefore, the development of a high-performance polypropylene composite material and its preparation method to meet higher performance requirements has become a current research hotspot. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present application provides a high-performance polypropylene composite material and a preparation method thereof. The high-performance polypropylene composite material of the present application has the advantages of excellent wear resistance, low linear expansion coefficient, excellent mechanical properties and excellent appearance, and is widely used in the fields of automobiles, home appliances, electronic products, etc., especially in parts requiring high wear resistance, low linear expansion coefficient and good surface appearance.
[0004] In the first aspect, the present application provides a high-performance polypropylene composite material, which adopts the following technical solution: A high-performance polypropylene composite material, wherein the raw materials for preparation include, by weight: 80-90 parts of a low melt mass flow rate PP resin, 4-4.5 parts of a high melt mass flow rate PP resin, 2-3 parts of a compatibilizer, 8-10 parts of modified basalt fibers, 4-6 parts of modified magnesium sulfate whiskers, 0.1-0.3 parts of an antioxidant, and 0.2-0.3 parts of a coupling agent, wherein the weight ratio of the low melt mass flow rate PP resin to the high melt mass flow rate PP resin is 20:1.
[0005] By adopting the above technical scheme, low melt mass flow rate PP resin and high melt mass flow rate PP resin: as the matrix of the composite material, provide the mechanical properties and processing properties of the material. Low melt mass flow rate PP resin has a higher molecular weight and can provide good mechanical properties; while high melt mass flow rate PP resin has a lower molecular weight and can improve the processing flow properties of the material. The ratio of the two is 20:1, which can improve the processing properties of the material while ensuring the mechanical properties of the material. Compatibilizer: improves the compatibility between modified basalt fiber and polypropylene, enhances the bonding force between the two, and thus improves the overall performance of the composite material. Modified basalt fiber: basalt fiber treated with a coupling agent and coated with zinc sulfide nanosheets has excellent mechanical properties and wear resistance. Zinc sulfide nanosheets can improve the bonding strength between the fiber and the polypropylene matrix and promote the transfer of stress between the two, thereby improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material. Modified magnesium sulfate whiskers: modified by γ-isocyanatepropyltriethoxysilane to improve its dispersibility and interfacial compatibility with the resin matrix, thereby improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material. Antioxidant: prevents oxidative degradation of polypropylene during processing and maintains the stability of the material's performance. Coupling agent: used for surface treatment of modified basalt fiber to provide an amine-based coupling agent layer on its surface, thereby improving the adsorption of zinc sulfide on the fiber surface and thus improving the stability of zinc sulfide nanosheets on the fiber. In summary, the high-performance polypropylene composite material in this application achieves the advantages of excellent wear resistance, low linear expansion coefficient, excellent mechanical properties and good appearance through the synergistic effect of each component, and is widely used in the fields of automobiles, home appliances, electronic products, etc.
[0006] Preferably, the low melt mass flow rate PP resin has a melt flow rate of 100 g / 10 min under the test conditions of 230° C. and 2.16 kg.
[0007] Preferably, the high melt mass flow rate PP resin has a melt flow rate of 150 g / 10 min under the test conditions of 230° C. and 2.16 kg.
[0008] By adopting the above technical solution, the inventors found that in the injection molding process of high-performance polypropylene composite materials, adding a specific proportion of high melt mass flow rate PP resin components will preferentially migrate to the surface of the product, thereby effectively inhibiting the exposure behavior of the modified basalt fiber, thereby improving the appearance quality and obtaining a product with excellent appearance.
[0009] Preferably, the method for preparing the modified basalt fiber comprises the following steps: S41. According to the mass fraction, 100 parts of basalt fibers with a diameter of 5-7 μm and an aspect ratio of 20-25 are placed in 500 parts of a sodium hydroxide solution with a mass concentration of 50 g / L for immersion treatment for 60-70 min, washed and dried after being taken out, and then placed in an ethanol / water solution containing 3-aminopropyltrimethoxysilane, and after standing for 3-4 hours, taken out, and dried at 100° C. for 1-2 hours to obtain 3-aminopropyltrimethoxysilane-modified basalt fibers; S42. Place 3-aminopropyltrimethoxysilane modified basalt fiber in a zinc sulfate aqueous solution, add triethylamine to adjust the pH to 2.5-3, then add sodium thiosulfate aqueous solution, heat to 93°C, keep warm for 2-3 hours, rinse and dry to obtain modified basalt fiber composite fiber.
[0010] By adopting the above technical solution, basalt fiber is a cylindrical inorganic substance with a large number of highly polar silanol groups on its surface. It has poor compatibility with polypropylene when directly mixed. If it is simply physically mixed under the action of external force, the composite effect is poor, and it is easy to have debonding at the two-phase interface, serious basalt fiber pull-out, matrix fracture, etc., so it cannot achieve the ideal reinforcement effect. The modified basalt fiber is treated by soaking the basalt fiber with 3-aminopropyltrimethoxysilane to form a coupling agent layer with amine groups on the fiber surface. On this basis, an in-situ chemical reaction method is used to generate zinc sulfide nanosheets on the fiber surface, and then the basalt fiber coated with zinc sulfide nanosheets on the surface is blended with polypropylene to prepare a reinforced composite material. The basalt fiber treated with 3-aminopropyltrimethoxysilane has a large number of amine atoms, which makes it have strong electron-accepting properties. It can produce a strong complexation effect on zinc ions and improve the adsorption of zinc sulfide on the fiber surface. At the same time, the zinc ions in zinc sulfide can also produce complexation with the anhydride groups in maleic anhydride grafted polypropylene, so that there is a strong interaction between the basalt fiber coated with zinc sulfide nanosheets and the polypropylene matrix, thereby improving the bonding strength between the organic matrix and the inorganic matrix, promoting the transfer of stress between the two, and effectively improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material. Zinc sulfide nanosheets have the characteristics of small volume and large specific area, and can be filled on the fiber surface to improve the interface bonding between basalt fiber and polypropylene matrix; on the other hand, nanosheets can increase the roughness of the fiber surface and increase the mechanical interlocking effect between basalt fiber and matrix. In addition, nanoparticles can also reduce the agglomeration between fibers, increase the contact area with the resin matrix, thereby improving the dispersibility of basalt fiber and the interface compatibility with the resin matrix.
[0011] Preferably, in step S41, the mass concentration of 3-aminopropyltrimethoxysilane in the ethanol / water solution of 3-aminopropyltrimethoxysilane is 1-2%, the pH is 3.8, and the volume ratio of ethanol to water in the ethanol / water solution is 9:1.
[0012] Preferably, in step S42, the mass concentration of the zinc sulfate aqueous solution is 4%-6%, the mass concentration of the sodium thiosulfate aqueous solution is 2%-3%, and the volume of the zinc sulfate aqueous solution is the same as that of the sodium thiosulfate aqueous solution.
[0013] Preferably, the method for preparing the modified magnesium sulfate whisker comprises the following steps: S71, adding 500 parts of magnesium sulfate whiskers having a diameter of 3-5 μm and an aspect ratio of 10-12 and 200 parts of calcium peroxide to 550 parts of a phosphoric acid solution having a mass concentration of 6 g / L, continuing the reaction for 30-40 min, then filtering and drying to obtain hydroxylated magnesium sulfate whiskers; S72, according to the mass fraction, add 8 parts of γ-isocyanatepropyltriethoxysilane to a mixture of 200 parts of ethanol and 30 parts of water, mix well, raise the temperature to 38° C., and hydrolyze for 200 minutes to obtain a mixture A; S73. Add the hydroxylated magnesium sulfate whisker into the mixed solution A, stir thoroughly, heat to 60° C., react for 90 min, filter, dry, crush and sieve to obtain modified magnesium sulfate whisker.
[0014] By adopting the above technical scheme, magnesium sulfate whisker (a brittle material with high strength and high modulus, has the characteristic of not increasing melt viscosity when mixed with polymer. The modified magnesium sulfate whisker is modified by γ-isocyanatepropyltriethoxysilane to improve its dispersibility and interface compatibility with the resin matrix, thereby improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material.
[0015] Preferably, the coupling agent is composed of 3-aminopropyltrimethoxysilane and γ-isocyanatepropyltriethoxysilane in a mass ratio of 3:4.
[0016] By adopting the above technical scheme, 3-aminopropyltrimethoxysilane (APTMS): APTMS molecules contain amino groups (-NH2), which can react with the silanol groups on the surface of basalt fibers to form stable chemical bonds, thereby improving the adhesion between basalt fibers and polypropylene. In addition, the methoxy groups (-OCH3) in APTMS can react chemically with polypropylene to further enhance the interfacial bonding force. γ-isocyanatepropyltriethoxysilane (IPTS): The isocyanate groups (-NCO) in IPTS can react with the hydroxyl or carboxyl groups on the polypropylene chain to form urea bonds or carbamate bonds, thereby enhancing interfacial interactions. Ethoxy groups (-OC2H5) can also react chemically with polypropylene to promote better interfacial compatibility. When these two coupling agents are used together, they can form a mixed coupling agent layer on the surface of basalt fibers and magnesium sulfate whiskers, which can not only improve the adhesion between inorganic fillers and polypropylene, but also promote the interaction between zinc sulfide nanosheets and polypropylene, thereby improving the performance of the composite material as a whole. In summary, by using APTMS and IPTS in a specific ratio as coupling agents, effective modification of basalt fibers and magnesium sulfate whiskers can be achieved, thereby greatly improving the wear resistance, mechanical properties and appearance quality of the composite materials, making them widely used in the fields of automobiles, home appliances, electronic products, etc.
[0017] Preferably, the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a mass ratio of 3:1; the compatibilizer is maleic anhydride grafted polypropylene with a grafting rate of 1%.
[0018] In a second aspect, the present application provides a method for preparing a high-performance polypropylene composite material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned high-performance polypropylene composite material, comprising the following steps: S101, adding low melt mass flow rate PP resin, high melt mass flow rate PP resin, compatibilizer, modified basalt fiber, modified magnesium sulfate whisker, antioxidant and coupling agent into a high-speed mixer according to the mass fractions, mixing them evenly to obtain a mixture; S102. Add the mixed material into the hopper of a twin-screw extruder, extrude, shear and granulate through the twin-screw extruder to obtain a high-performance polycarbonate composite material, wherein the screw diameter is 60 mm, the aspect ratio of the screw is 39:1, and the temperatures of the screw zones are: 180° C. in the first zone, 190° C. in the second zone, 200° C. in the third zone, 210° C. in the fourth zone, 220° C. in the fifth zone, and 210° C. in the sixth zone.
[0019] In summary, the present application includes at least one of the following beneficial technical effects: The high-performance polypropylene composite material of the present application effectively inhibits the exposure behavior of the modified basalt fiber and improves the appearance quality of the product by adding a high melt mass flow rate PP resin component in a specific proportion. At the same time, the introduction of modified basalt fiber and modified magnesium sulfate whisker improves the wear resistance, linear expansion coefficient and mechanical properties of the composite material.
[0020] After the basalt fiber is treated with a coupling agent, an amine-containing coupling agent layer is formed on the fiber surface, and zinc sulfide nanosheets are generated by an in-situ chemical reaction method. This treatment method allows a strong interaction between the basalt fiber and the polypropylene matrix, improves the bonding strength between the organic matrix and the inorganic matrix, promotes the transfer of stress between the two, and effectively improves the wear resistance, linear expansion coefficient and mechanical properties of the composite material. In addition, the stable adsorption of zinc sulfide nanosheets on the surface of basalt fibers and their complexation with maleic anhydride grafted polypropylene further enhance the bonding strength between the organic matrix and the inorganic matrix, promotes the transfer of stress between the two, and effectively improves the performance of the composite material.
[0021] The addition of modified magnesium sulfate whiskers, due to its high strength and high modulus characteristics, does not increase the melt viscosity, and further improves the wear resistance, linear expansion coefficient and mechanical properties of the composite material.
[0022] In general, the high-performance polypropylene composite material of the present application has the advantages of excellent wear resistance, low linear expansion coefficient, excellent mechanical properties and good surface appearance, and can be widely used in the fields of automobiles, home appliances, electronic products, etc., especially in parts requiring high wear resistance, low linear expansion coefficient and good surface appearance. DETAILED DESCRIPTION
[0023] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If no specific conditions are specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased from the market. Antioxidant 1010, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, was purchased from BASF; antioxidant 1076, n-octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, was purchased from BASF; low melt mass flow rate PP resin was purchased from Sinopec Yangzi Petrochemical Co., Ltd., with the grade YPJ3100H (melt flow rate of 100 g / 10 min under the test conditions of 30°C and 2.16 kg), and high melt mass flow rate PP resin was purchased from LG Chemical Co., Ltd. of South Korea, with the grade MH7900 (melt flow rate of 150 g / 10 min under the test conditions of 230°C and 2.16 kg).
[0024] Preparation Example 1 Preparation of modified basalt fiber The preparation method of modified basalt fiber comprises the following steps: S41. According to the mass fraction, 100 g of basalt fiber with a diameter of 5-7 μm and an aspect ratio of 20-25 is placed in 500 g of a sodium hydroxide solution with a mass concentration of 50 g / L for 60 min, washed and dried after being taken out, and then placed in an ethanol / water solution (the volume ratio of ethanol to water is 9:1) containing 3-aminopropyltrimethoxysilane with a mass concentration of 1% and a pH of 3.8, and then taken out after standing for 4 hours, and dried at 100° C. for 1 hour to obtain 3-aminopropyltrimethoxysilane-modified basalt fiber; S42. Place 3-aminopropyltrimethoxysilane modified basalt fiber in 1L of 4% zinc sulfate aqueous solution, add triethylamine to adjust the pH to 2.5, then add 1L of 2% sodium thiosulfate aqueous solution, heat to 93°C, keep warm for 2h, rinse and dry to obtain modified basalt fiber composite fiber.
[0025] Preparation Example 2 Preparation of modified basalt fiber The preparation method of modified basalt fiber comprises the following steps: S41. According to the mass fraction, 100 g of basalt fiber with a diameter of 5-7 μm and an aspect ratio of 20-25 is placed in 500 g of a sodium hydroxide solution with a mass concentration of 50 g / L for 70 min, washed and dried after being taken out, and then placed in an ethanol / water solution (the volume ratio of ethanol to water is 9:1) containing 3-aminopropyltrimethoxysilane with a mass concentration of 2% and a pH of 3.8, and then taken out after standing for 3 hours, and dried at 100° C. for 2 hours to obtain 3-aminopropyltrimethoxysilane-modified basalt fiber; S42. Place 3-aminopropyltrimethoxysilane modified basalt fiber in 1L of 6% zinc sulfate aqueous solution, add triethylamine to adjust the pH to 3, then add 1L of 3% sodium thiosulfate aqueous solution, heat to 93°C, keep warm for 3h, rinse and dry to obtain modified basalt fiber composite fiber.
[0026] Preparation Example 3 Preparation of modified basalt fiber The preparation method of modified basalt fiber comprises the following steps: S41. According to the mass fraction, 100 g of basalt fiber with a diameter of 5-7 μm and an aspect ratio of 20-25 is placed in 500 g of a sodium hydroxide solution with a mass concentration of 50 g / L for 65 min, washed and dried after being taken out, and then placed in an ethanol / water solution (the volume ratio of ethanol to water is 9:1) containing 3-aminopropyltrimethoxysilane with a mass concentration of 1.5% and a pH of 3.8, and then taken out after standing for 3.5 hours, and dried at 100° C. for 1.5 hours to obtain 3-aminopropyltrimethoxysilane-modified basalt fiber; S42. Place 3-aminopropyltrimethoxysilane modified basalt fiber in 1L of 5% zinc sulfate aqueous solution, add triethylamine to adjust the pH to 2.8, then add 1L of 2.5% sodium thiosulfate aqueous solution, heat to 93°C, keep warm for 2.5h, rinse and dry to obtain modified basalt fiber composite fiber.
[0027] Preparation Example 4 Preparation of modified magnesium sulfate whiskers The preparation method of modified magnesium sulfate whisker comprises the following steps: S71, according to the mass fractions, add 500g of magnesium sulfate whiskers with a diameter of 3-5μm and an aspect ratio of 10-12 and 200g of calcium peroxide to 550g of a phosphoric acid solution with a mass concentration of 6g / L, continue the reaction for 35min, then filter and dry to obtain hydroxylated magnesium sulfate whiskers; S72, according to the mass fraction, add 8 g of γ-isocyanatepropyltriethoxysilane to a mixture of 200 g of ethanol and 30 g of water, mix well, heat to 38° C., and hydrolyze for 200 minutes to obtain a mixture A; S73. Add the hydroxylated magnesium sulfate whisker into the mixed solution A, stir thoroughly, heat to 60° C., react for 90 min, filter, dry, crush and sieve to obtain modified magnesium sulfate whisker.
[0028] Example 1 A high-performance polypropylene composite material, wherein the raw materials for preparation include, by weight: 800 g of a low melt mass flow rate PP resin, 40 g of a high melt mass flow rate PP resin, 20 g of maleic anhydride grafted polypropylene (grafting rate is 1%), 80 g of modified basalt fiber, 60 g of modified magnesium sulfate whisker, 1 g of an antioxidant, and 2 g of a coupling agent, wherein the coupling agent is composed of 3-aminopropyltrimethoxysilane and γ-isocyanatepropyltriethoxysilane in a weight ratio of 3:4, the modified basalt fiber is prepared according to Preparation Example 1, and the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1; The method for preparing the high-performance polypropylene composite material comprises the following steps: S101, adding low melt mass flow rate PP resin, high melt mass flow rate PP resin, maleic anhydride grafted polypropylene (grafting rate is 1%), modified basalt fiber, modified magnesium sulfate whisker, antioxidant and coupling agent into a high-speed mixer according to mass parts, mixing them evenly to obtain a mixture; S102. Add the mixed material into the hopper of a twin-screw extruder, extrude, shear and granulate through the twin-screw extruder to obtain a high-performance polycarbonate composite material, wherein the screw diameter is 60 mm, the aspect ratio of the screw is 39:1, and the temperatures of the screw zones are: 180° C. in the first zone, 190° C. in the second zone, 200° C. in the third zone, 210° C. in the fourth zone, 220° C. in the fifth zone, and 210° C. in the sixth zone.
[0029] Example 2 A high-performance polypropylene composite material, wherein the raw materials for preparation include, by weight: 900 g of a low melt mass flow rate PP resin, 45 g of a high melt mass flow rate PP resin, 30 g of maleic anhydride grafted polypropylene (grafting rate is 1%), 100 g of modified basalt fiber, 40 g of modified magnesium sulfate whisker, 3 g of an antioxidant, and 3 g of a coupling agent, wherein the coupling agent is composed of 3-aminopropyltrimethoxysilane and γ-isocyanatepropyltriethoxysilane in a weight ratio of 3:4, the modified basalt fiber is prepared in Preparation Example 2, and the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1; a method for preparing the above-mentioned high-performance polypropylene composite material comprises the following steps: S101, adding low melt mass flow rate PP resin, high melt mass flow rate PP resin, maleic anhydride grafted polypropylene (grafting rate is 1%), modified basalt fiber, modified magnesium sulfate whisker, antioxidant and coupling agent into a high-speed mixer according to mass parts, mixing them evenly to obtain a mixture; S102. Add the mixed material into the hopper of a twin-screw extruder, extrude, shear and granulate through the twin-screw extruder to obtain a high-performance polycarbonate composite material, wherein the screw diameter is 60 mm, the aspect ratio of the screw is 39:1, and the temperatures of the screw zones are: 180° C. in the first zone, 190° C. in the second zone, 200° C. in the third zone, 210° C. in the fourth zone, 220° C. in the fifth zone, and 210° C. in the sixth zone.
[0030] Example 3 A high-performance polypropylene composite material, the raw materials for preparation include, by weight: 860g of a low melt mass flow rate PP resin, 43g of a high melt mass flow rate PP resin, 25g of maleic anhydride grafted polypropylene (grafting rate is 1%), 90g of modified basalt fiber, 50g of modified magnesium sulfate whisker, 2g of an antioxidant, and 2.5g of a coupling agent, wherein the coupling agent is composed of 3-aminopropyltrimethoxysilane and γ-isocyanatepropyltriethoxysilane in a weight ratio of 3:4, the modified basalt fiber is prepared in Preparation Example 3, and the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1; the preparation method of the above-mentioned high-performance polypropylene composite material comprises the following steps: S101, adding low melt mass flow rate PP resin, high melt mass flow rate PP resin, maleic anhydride grafted polypropylene (grafting rate is 1%), modified basalt fiber, modified magnesium sulfate whisker, antioxidant and coupling agent into a high-speed mixer according to mass parts, mixing them evenly to obtain a mixture; S102. Add the mixed material into the hopper of a twin-screw extruder, extrude, shear and granulate through the twin-screw extruder to obtain a high-performance polycarbonate composite material, wherein the screw diameter is 60 mm, the aspect ratio of the screw is 39:1, and the temperatures of the screw zones are: 180° C. in the first zone, 190° C. in the second zone, 200° C. in the third zone, 210° C. in the fourth zone, 220° C. in the fifth zone, and 210° C. in the sixth zone.
[0031] Comparative Example 1 The same as Example 3, except that: 903g of low melt mass flow rate PP resin and 0g of high melt mass flow rate PP resin.
[0032] Comparative Example 2 The same as Example 3, except that: the coupling agent is 3-aminopropyltrimethoxysilane.
[0033] Comparative Example 3 The same as Example 3, except that: the coupling agent is γ-isocyanatepropyltriethoxysilane.
[0034] Comparative Example 4 The same as Example 3, except that: basalt fibers with an equivalent diameter of 5-7 μm and an aspect ratio of 20-25 are used instead of the modified basalt fibers prepared in Preparation Example 3.
[0035] Comparative Example 5 The same as Example 3, except that magnesium sulfate whiskers with an equivalent diameter of 3-5 μm and an aspect ratio of 10-12 are used instead of the modified magnesium sulfate whiskers prepared in Preparation Example 4.
[0036] Performance testing The high-performance polypropylene composite materials prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were sampled and injection molded into test plates for testing. The test results are shown in Table 1. Tensile strength: Test the material tensile strength according to the IS0527 test method, the test condition is 50mm / min, the unit is MPa; Notched impact strength: Test the material notched impact strength according to the ISO179 test method, the test condition is 23℃, the unit is kJ / m 2 ; Shrinkage rate: Tested according to ISO 294 method. The post-shrinkage test condition is to test the sample 48 hours after injection molding. The test unit is %; Shrinkage rate after heat treatment at 90℃: tested according to ISO294 method. The shrinkage test condition is that the sample is heat treated at 90℃ for 48 hours after injection molding and then cooled to room temperature for 48 hours before testing. The test unit is %; Linear expansion coefficient: tested according to ISO11359 method, test conditions are -30-110℃, sample size is 10*10*4mm, test unit is 10 -6 mm / mm / ℃, the test direction is the flow direction.
[0037] Surface appearance: injection molding 150*100*3mm smooth board, evaluate the surface appearance of the smooth board, mainly focusing on whether the surface is smooth, whether there are floating fibers and other appearance defects; Wear resistance test: Tested according to GMW14688 method, 10N, 100-grid cross scratch.
[0038] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The high-performance polypropylene composite materials prepared in Examples 1 to 3 have the advantages of excellent wear resistance, low linear expansion coefficient, excellent mechanical properties and excellent appearance, and are widely used in the fields of automobiles, home appliances, electronic products, etc.
[0039] 2) The comparative analysis of the performance of the high-performance polypropylene composite material obtained in combination with Example 3 and Comparative Example 1 shows that during the injection molding process of the high-performance polypropylene composite material, the addition of a specific proportion of the high melt mass flow rate PP resin component will preferentially migrate to the surface of the product, thereby effectively inhibiting the exposure of the modified basalt fiber, thereby improving the appearance quality and obtaining a product with excellent appearance.
[0040] 3) A comparative analysis of the performance of the high-performance polypropylene composite materials obtained in combination with Example 3 and Comparative Examples 2-3 shows that the coupling agent is composed of 3-aminopropyltrimethoxysilane and γ-isocyanatepropyltriethoxysilane in a mass ratio of 3:4. By utilizing the synergistic effect between them, the wear resistance, mechanical properties and appearance quality of the composite material are greatly improved, and the linear expansion coefficient is reduced.
[0041] 4) The performance comparison analysis of the high-performance polypropylene composite material prepared in combination with Example 3 and Comparative Example 4 shows that the modified basalt fiber prepared in this application is treated by soaking the basalt fiber with 3-aminopropyltrimethoxysilane to form a coupling agent layer with an amine group on the fiber surface. On this basis, an in-situ chemical reaction method is used to generate zinc sulfide nanosheets on the fiber surface, and then the basalt fiber coated with zinc sulfide nanosheets on the surface is blended with polypropylene to prepare a reinforced composite material. The basalt fiber treated with 3-aminopropyltrimethoxysilane has a large number of amine atoms, which makes it have a strong electron-accepting property. It can produce a strong complexation effect on zinc ions and improve the adsorption of zinc sulfide on the fiber surface. At the same time, the zinc ions in zinc sulfide can also produce a complexation effect with the anhydride groups in maleic anhydride grafted polypropylene, so that the basalt fiber coated with zinc sulfide nanosheets and the polypropylene matrix have a strong interaction, thereby improving the bonding strength between the organic matrix and the inorganic matrix, promoting the transmission of stress between the two, and then effectively improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material.
[0042] 5) A comparative analysis of the performance of the high-performance polypropylene composite material prepared in combination with Example 3 and Comparative Example 5 shows that the modified magnesium sulfate whiskers prepared in the present application are modified by γ-isocyanatepropyltriethoxysilane to improve their dispersibility and interfacial compatibility with the resin matrix, thereby improving the wear resistance, linear expansion coefficient and mechanical properties of the composite material.
[0043] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. A high performance polypropylene composite material, characterized in that: Calculated by weight, the raw materials include: 80-90 parts of low melt mass flow rate PP resin, 4-4.5 parts of high melt mass flow rate PP resin, 2-3 parts of compatibilizer, 8-10 parts of modified basalt fiber, 4-6 parts of modified magnesium sulfate whisker, 0.1-0.3 parts of antioxidant, and 0.2-0.3 parts of coupling agent, wherein the mass ratio of the low melt mass flow rate PP resin to the high melt mass flow rate PP resin is 20:
1.
2. A high performance polypropylene composite material according to claim 1, characterized in that: The low melt mass flow rate PP resin has a melt flow rate of 100 g / 10 min under the test conditions of 230° C. and 2.16 kg.
3. A high performance polypropylene composite material according to claim 1, characterized in that: The high melt mass flow rate PP resin has a melt flow rate of 150 g / 10 min under the test conditions of 230° C. and 2.16 kg.
4. A high performance polypropylene composite material according to claim 1, characterized in that: The preparation method of the modified basalt fiber comprises the following steps: S41. According to the mass fraction, 100 parts of basalt fibers with a diameter of 5-7 μm and an aspect ratio of 20-25 are placed in 500 parts of a sodium hydroxide solution with a mass concentration of 50 g / L for immersion treatment for 60-70 min, washed and dried after being taken out, and then placed in an ethanol / water solution containing 3-aminopropyltrimethoxysilane, left to stand for 34 hours, and then taken out, and dried at 100° C. for 1-2 hours to obtain 3-aminopropyltrimethoxysilane-modified basalt fibers; S42. Place 3-aminopropyltrimethoxysilane modified basalt fiber in a zinc sulfate aqueous solution, add triethylamine to adjust the pH to 2.5-3, then add sodium thiosulfate aqueous solution, heat to 93°C, keep warm for 2-3 hours, rinse and dry to obtain modified basalt fiber composite fiber.
5. A high performance polypropylene composite material according to claim 4, characterized in that: In step S41, the mass concentration of 3-aminopropyltrimethoxysilane in the ethanol / water solution of 3-aminopropyltrimethoxysilane is 1-2%, the pH is 3.8, and the volume ratio of ethanol to water in the ethanol / water solution is 9:
1.
6. A high performance polypropylene composite material according to claim 4, characterized in that: In step S42, the mass concentration of the zinc sulfate aqueous solution is 4%-6%, the mass concentration of the sodium thiosulfate aqueous solution is 2%-3%, and the volume of the zinc sulfate aqueous solution is the same as that of the sodium thiosulfate aqueous solution.
7. A high performance polypropylene composite material according to claim 1, characterized in that: The preparation method of the modified magnesium sulfate whisker comprises the following steps: S71, adding 500 parts of magnesium sulfate whiskers having a diameter of 3-5 μm and an aspect ratio of 10-12 and 200 parts of calcium peroxide to 550 parts of a phosphoric acid solution having a mass concentration of 6 g / L, continuing the reaction for 30-40 min, then filtering and drying to obtain hydroxylated magnesium sulfate whiskers; S72, according to the mass fraction, add 8 parts of γ-isocyanatepropyltriethoxysilane to a mixture of 200 parts of ethanol and 30 parts of water, mix well, raise the temperature to 38° C., and hydrolyze for 200 minutes to obtain a mixture A; S73. Add the hydroxylated magnesium sulfate whisker into the mixed solution A, stir thoroughly, heat to 60° C., react for 90 min, filter, dry, crush and sieve to obtain modified magnesium sulfate whisker.
8. The high performance polypropylene composite material according to claim 1, characterized in that: The coupling agent is composed of 3-aminopropyltrimethoxysilane and gamma-isocyanatepropyltriethoxysilane in a mass ratio of 3:
4.
9. The high performance polypropylene composite material according to claim 1, characterized in that: The antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a mass ratio of 3:1; the compatibilizer is maleic anhydride grafted polypropylene with a grafting rate of 1%.
10. A method for preparing a high-performance polypropylene composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, adding low melt mass flow rate PP resin, high melt mass flow rate PP resin, compatibilizer, modified basalt fiber, modified magnesium sulfate whisker, antioxidant and coupling agent into a high-speed mixer according to the mass fractions, mixing them evenly to obtain a mixture; S102. Add the mixed material into the hopper of a twin-screw extruder, extrude, shear and granulate through the twin-screw extruder to obtain a high-performance polycarbonate composite material, wherein the screw diameter is 60 mm, the aspect ratio of the screw is 39:1, and the temperatures of the screw zones are: 180° C. in the first zone, 190° C. in the second zone, 200° C. in the third zone, 210° C. in the fourth zone, 220° C. in the fifth zone, and 210° C. in the sixth zone.
Citation Information
Cited By
Anti-ultraviolet, corrosion-resistant, low-temperature-resistant and anti-freezing geotextile material composition
CN121064564A
An ultraviolet resistant, corrosion resistant and low temperature resistant geotextile material composition
CN121064564B