Heat-sensitive recording material protection liquid as well as preparation method and application thereof
Through the combination of modified layered fluorosilicate and reactive polyvinyl alcohol, a tightly cross-linked protective film is formed, which solves the problem of stickiness and debris during high-energy printing of thermal recording materials and extends the length of the print head. It has a long lifespan and maintains image quality, meeting the requirements for high transmittance color density and clear details for medical imaging diagnosis.
Patent Information
- Application Number
- CN202410991705.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Existing thermal recording materials are prone to problems such as accumulation of adhesion on the film surface, accumulation of debris, wear of the print head, and degradation of image quality during high-energy printing. Especially when used continuously for a long time and in batches, they cannot meet the high transparency requirements of medical imaging diagnosis. Light color density, detail clarity, and contrast requirements.
Modified layered fluorosilicate is used as a functional barrier material, combined with reactive polyvinyl alcohol, lubricants and nanofillers, to form a tightly cross-linked protective film through chemical properties and physical structural properties, reducing the amount of lubricants and fillers. , improve the hardness and temperature resistance of the protective layer to prevent print head wear and image quality degradation.
It can reduce the precipitation of lubricants and fillers under high-energy printing conditions, extend the life of the print head, maintain clear image details and mirror gloss effects, meet the needs of long-term batch continuous use, and improve the image quality and service life of thermal recording materials. .
Smart Images

Figure BDA0004959049380000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermosensitive materials, and more specifically to a thermosensitive recording material protective liquid and a preparation method and application thereof. Background Art
[0002] With the development of thermal technology, thermal recording materials are often used as auxiliary consumables for medical imaging diagnosis. Dry thermal printing films are commonly used now. They are convenient, fast and efficient to use. They can be printed out instantly with a matching thermal printer, without darkroom operation and pollution-free developer. Due to the medical imaging diagnosis field, images are required to have high light transmittance and color concentration, clear details, and high contrast. The printing equipment used with the recording materials of this application is different from the general thermal label printer or POS machine. Its print head heating time is longer and the printing energy is extremely high (print head heating time exceeds 2 minutes, and printing energy exceeds 100mJ / mm 2 ), therefore, when thermal films are used in batches, the print heads are prone to accumulation of sticky matter on the film surface and accumulation of debris on the print heads, causing print head contamination. Long-term use will lead to wear of the print heads and shorten their service life. Thermal films are also prone to damage such as scratches, white stripes, black stripes, etc., affecting image quality and thus affecting the diagnosis of medical users.
[0003] Chinese patent CN111471508A prepares a lubricant and applies it to the protective layer of thermal recording materials. It has a good lubricating effect, thereby reducing the friction coefficient between the film and the print head during printing, thereby alleviating the precipitation of melt on the film surface during printing and reducing print head pollution. However, it can only ensure that there is no physical damage to the film surface when 100 sheets of film are printed continuously, and cannot meet the actual use needs of long-term and batch printing in hospitals. Chinese patent CN101247963A improves the problems of debris attached to the print head and damage to the print head during high-energy printing by using a variety of fillers such as aluminum hydroxide, kaolin, and silica, and achieves continuous use of 5,000 sheets of film; however, the surface of the high-concentration part is prone to roughness and the glossiness deteriorates, which has a negative impact on the overall image effect, and the haze is relatively unstable. The protective layer contains a relatively high proportion of lubricants and fillers (lubricants account for 18wt%, and fillers account for 15-23wt%).
[0004] At present, the existing technology mainly uses lubricants to improve the lubrication effect, reduce the friction between the print head and the film, and thus reduce the appearance of scratches. However, lubricants are easy to melt and precipitate when printing at high energy, causing foreign matter to accumulate on the print head and even causing the film protective layer to soften and break. Alternatively, different fillers are mainly matched with each other to reduce the precipitated substances or debris of the film protective layer during printing, thereby reducing the accumulation of foreign matter on the print head and extending the life of the print head. However, increasing the amount of fillers will make the transparency worse and the high-concentration color development area rough and matte, affecting the image effect.
[0005] Therefore, there is an urgent need to develop a thermal recording material that can be used for a long time and continuously in batches, with a small amount of lubricant and filler, and is particularly suitable for print heads with long heating time and high printing energy. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a thermal recording material protective liquid, a preparation method and an application thereof. The present invention uses a modified layered fluorinated silicate as a functional barrier material to prepare a thermal recording material protective liquid, thereby greatly reducing the amount of lubricant and filler (the lubricant only accounts for 3-8wt%, and the nanofiller only accounts for 5-10wt%), and the thermal recording material protective liquid is further used to prepare a protective layer of the thermal recording material. By means of the chemical properties, physical structure properties, and auxiliary cross-linking and hardening effect of the modified layered fluorinated silicate and polyvinyl alcohol, the continuous film-forming and hardening effect of the protective layer is enhanced, and the hardness and temperature resistance of the protective layer are improved, so that the thermal recording material also exhibits a good mirror gloss effect in the high concentration area after printing, thereby ensuring the best embodiment of the image effect.
[0007] A first aspect of the present invention provides a heat-sensitive recording material protecting liquid.
[0008] Specifically, a heat-sensitive recording material protective liquid comprises the following raw materials in parts by weight:
[0009] 40-90 parts of reactive polyvinyl alcohol,
[0010] 1-8 parts of the first cross-linking hardener,
[0011] 3-18 parts of aqueous dispersion of functional barrier material,
[0012] 3-8 parts of lubricant,
[0013] Nano filler 5-10 parts,
[0014] 5-15 parts of self-crosslinking reaction latex,
[0015] Wetting and leveling agent 0.5-5 parts;
[0016] The functional barrier material aqueous dispersion contains modified layered fluorine-containing silicate with a particle size of less than or equal to 100 nm and a stabilizer.
[0017] The present invention utilizes the layered structure and nanometer-scale particle size of the modified layered fluorine-containing silicate to achieve good barrier effect while ensuring good transparency, preventing excessive precipitation of molten materials such as lubricants or the formation of filler debris on the film surface during high-energy printing, resulting in wear of the print head. The thermal recording material protective liquid is further used to prepare the film protective layer, and the modified layered fluorine-containing silicate can reduce the dependence of the protective layer on lubricants and conventional large amounts of fillers (in the present invention, the lubricant only accounts for 3-8wt%, and the nano filler only accounts for 5-10wt%), while ensuring that the wear of the print head is reduced. In addition, the modified layered fluorine-containing silicate can also form a continuous film (because of its layered structure, the particles can form an association effect between edges and faces, edges and edges, and faces and faces, and at the same time, under the action of van der Waals force, the particles are connected to each other, thereby forming a continuous film), and form a tightly cross-linked protective film surface with the reactive polyvinyl alcohol glue, strengthen the cross-linking and hardening film-forming effect of polyvinyl alcohol, make the protective layer stronger and more resistant to high temperature, not easy to soften and be damaged during printing, not easy to form physical scratches or stripes, and can always maintain a good mirror gloss effect, clear image details and good image quality during continuous batch printing of images with different printing energies and different printing densities.
[0018] Preferably, the thermal recording material protective liquid comprises the following raw materials in parts by weight:
[0019] Reactive polyvinyl alcohol 50-80 parts,
[0020] 1-5 parts of the first cross-linking hardener,
[0021] 3-15 parts of aqueous dispersion of functional barrier material,
[0022] 3-8 parts of lubricant,
[0023] Nano filler 5-10 parts,
[0024] 5-15 parts of self-crosslinking reaction latex,
[0025] 0.5-2 parts of wetting and leveling agent.
[0026] Preferably, when the solid content of the functional barrier material aqueous dispersion is 10%, the functional barrier material aqueous dispersion contains 90-95% of the modified layered fluorine-containing silicate and 5-10% of the stabilizer by weight. The modified layered fluorine-containing silicate and the stabilizer are mixed and dispersed in the functional barrier material aqueous dispersion to improve its dispersion effect and stability, so that its mixed compatibility and dispersion effect in the protective liquid remain stable and good, and no gel problem occurs, resulting in a poor protective layer effect.
[0027] Preferably, the viscosity of the aqueous dispersion of the functional barrier material is less than 100 mp.s.
[0028] Preferably, the stabilizer is polyvinyl alcohol and / or pyrophosphate (such as tetrasodium pyrophosphate).
[0029] Preferably, the degree of polymerization of the polyvinyl alcohol is ≤500, and / or the viscosity of the polyvinyl alcohol is ≤10 mPa.s. Polyvinyl alcohol has low viscosity and low degree of polymerization.
[0030] Preferably, the modified layered fluorine-containing silicate is a modified layered fluorine-containing silicate of BYK Chemical Model S and / or a modified layered fluorine-containing silicate of BYK Chemical Model JS. The specific modified layered fluorine-containing silicate selected in the present invention has a layered structure, a nano-scale particle size and fluorine-containing properties, so that the protective layer prepared therefrom has excellent barrier effect and anti-sticking effect.
[0031] Preferably, the reactive polyvinyl alcohol is at least one of carboxyl-modified reactive polyvinyl alcohol, acetoacetyl-modified reactive polyvinyl alcohol, silane-modified reactive polyvinyl alcohol, and diacetone-modified reactive polyvinyl alcohol.
[0032] Preferably, the polymerization degree of the reactive polyvinyl alcohol is 1700-3500. While ensuring that the aqueous protective liquid is suitable for the viscosity range, the reaction film strength also meets the requirements, and the film strength and density after the reaction are good, so that the coating can have good heat resistance, scratch resistance, physical scratch resistance, and a certain water resistance.
[0033] Preferably, the first cross-linking hardener is at least one of polyamide epichlorohydrin resin, polyaziridine, polycarbodiimide, adipic acid dihydrazide, and aldehyde cross-linking hardener (molecular weight within 120). The first cross-linking hardener can react with modified or unmodified polyvinyl alcohol.
[0034] Preferably, the weight of the first cross-linking hardener accounts for 1.25-20% of the weight of the reactive polyvinyl alcohol.
[0035] Further preferably, the weight of the first cross-linking hardener accounts for 2-10% of the weight of the reactive polyvinyl alcohol.
[0036] Preferably, the reaction conditions of the first cross-linking hardener and reactive polyvinyl alcohol are: temperature 30-60°C, relative humidity 30-70% RH, and time more than 24 hours. The above conditions can ensure a more complete cross-linking densification effect and a more scratch-resistant physical basic property. The above-mentioned functional barrier material, due to its modified fluorine-containing silicate chemical properties and the physical properties of the layered structure, can cooperate with the reactive polyvinyl alcohol in the protective liquid to form a better coherent film-forming effect. After coating and drying, the surface is delicate and smooth, and it helps to strengthen the reaction effect of the first cross-linking hardener and the reactive polyvinyl alcohol, shortening the reaction time to less than 24 hours, making the film layer of the protective layer denser, harder, scratch-resistant, and temperature-resistant.
[0037] Preferably, the lubricant is at least one of a fatty acid salt lubricant (such as at least one of calcium stearate, zinc stearate, stearic acid amide, diethylene stearate, oleic acid amide, and erucic acid amide), a silicone oil lubricant (such as at least one of dimethyl water-based silicone solution, anti-sticking emulsion silicone, and demolding modified silicone emulsion), and an aqueous paraffin emulsion (such as at least one of montan wax emulsion, palm wax emulsion, oxidized polyethylene wax emulsion, polytetrafluoroethylene wax emulsion, and microcrystalline nano wax emulsion). The above lubricants can be selected and used in combination to achieve a synergistic optimization of the lubrication effect, and an aqueous dispersion or aqueous solution with a particle size of less than 0.5 μm is more preferred to ensure good transparency of the thermal recording material and a bright protective layer surface visual effect.
[0038] Preferably, the nano filler is at least one of nano silicon dioxide, nano alumina, nano zirconium oxide, nano kaolin and nano silica sol.
[0039] Further preferably, the nanofiller is nano-silicon dioxide or nano-silica sol.
[0040] Preferably, the particle size of the nanofiller is ≤50nm. Small-particle nanofillers can ensure the excellent transparency of heat-sensitive materials; and have good dispersion and compatibility effects, high temperature resistance and oil absorption properties, and can absorb part of the melted lubricant to prevent the molten material from adhering and accumulating on the print head during printing, which will cause black and white streaks or scratches after accumulation.
[0041] The above-mentioned functional barrier material, due to its barrier properties formed by its layered structure and dense continuous film-forming effect, can to a certain extent prevent the excessive precipitation of lubricant during printing, or the peeling of debris from the protective layer during printing, thereby reducing the use of fillers and playing a synergistic effect with the fillers in protecting the print head.
[0042] Preferably, the self-crosslinking latex is at least one of acrylic latex, styrene acrylic latex and polyurethane latex having self-crosslinking groups. The use of the self-crosslinking latex can make the protective layer and the imaging surface coating layer adhere better, avoid the bulging and foaming of the protective layer, and assist in strengthening the film-forming effect of the overall protective layer.
[0043] Preferably, the wetting and leveling agent is at least one of an organosilicon wetting and leveling agent, an alkyl sulfonate wetting and leveling agent, an acetylene alcohol wetting and leveling agent, and a fluorine wetting and leveling agent.
[0044] Preferably, the viscosity of the heat-sensitive recording material protection liquid is 20-80 mPa.s.
[0045] A second aspect of the present invention provides a method for preparing a heat-sensitive recording material protective liquid.
[0046] A method for preparing a thermal recording material protective liquid comprises the following steps:
[0047] Reactive polyvinyl alcohol and water are mixed and stirred, and an aqueous dispersion of a functional barrier material is added and mixed and stirred. A lubricant, a nanofiller, a self-crosslinking reactive latex, and a wetting and leveling agent are added in sequence and mixed and stirred. A first crosslinking hardener is added to prepare the thermal recording material protective liquid.
[0048] Preferably, the preparation method of the aqueous dispersion of the functional barrier material is as follows: the modified layered fluorinated silicate, water and a stabilizer are mixed and stirred at 10-40°C, the stirring speed is above 2500rpm, and the stirring time is 0.5-1h, to obtain the aqueous dispersion of the functional barrier material. An appropriate amount of stabilizer and a suitable dispersion temperature in the aqueous dispersion of the functional barrier material can ensure that the dispersion remains in a good low viscosity state, with a good dispersion effect. After the protective liquid is subsequently added, it can be better dispersed and compatible with other components to avoid gel agglomeration.
[0049] A third aspect of the present invention provides a heat-sensitive recording material.
[0050] A thermal recording material comprises a substrate, a thermal imaging top coating and a protective layer in sequence. The protective layer is obtained by coating a thermal recording material protective liquid once, and the thermal imaging top coating is coated on the front side of the substrate.
[0051] Preferably, the thermal recording material further comprises a primer connecting layer coated between the front side of the substrate and the thermal imaging top coating layer, and / or the thermal recording material further comprises a back coating layer coated on the back side of the substrate.
[0052] Preferably, the substrate is transparent polyethylene terephthalate (PET). The transparent support substrate used for the thermal recording material requires good flatness, small thermal deformation, high chemical stability, small stretchability or shrinkage, low haze, high transparency, and high stiffness, so transparent PET is selected.
[0053] Preferably, the thickness of the substrate is 150-180 μm.
[0054] Preferably, the back coating layer is obtained by coating a back coating layer coating liquid, and the back coating layer coating liquid includes the following raw materials: acrylic resin, polyurethane resin, silicon dioxide, silicone emulsion, paraffin emulsion, crosslinking agent, fluorocarbon surfactant and ultraviolet absorber.
[0055] Further preferably, the back coating coating liquid includes the following raw materials, measured in parts by weight: 40-60 parts of acrylic resin, 10-20 parts of polyurethane resin, 1-5 parts of silicon dioxide, 0.5-5 parts of silicone emulsion, 1-5 parts of paraffin emulsion, 1-3 parts of crosslinking agent, 0.5-1.5 parts of fluorocarbon surfactant, and 1-2 parts of ultraviolet absorber.
[0056] More preferably, the back coating coating liquid comprises the following raw materials, measured in parts by weight: 40 parts of acrylic resin, 10 parts of polyurethane resin, 1 part of silicon dioxide, 0.5 parts of silicone emulsion, 1 part of paraffin emulsion, 1 part of cross-linking agent, 0.5 parts of fluorocarbon surfactant, and 1 part of ultraviolet absorber.
[0057] Preferably, the method for preparing the back coating liquid comprises: mixing the raw materials, and then diluting the mixture with water as a medium to a solid content of 10%.
[0058] Preferably, the coating amount of the back coating is 20-30 mL / m 2 .
[0059] Preferably, the thermal imaging topcoat is obtained by coating a thermal imaging topcoat coating liquid, and the thermal imaging topcoat coating liquid includes the following raw materials: dye dispersion, developer dispersion, adhesive, second cross-linking hardener, defoamer, leveling agent and tackifier.
[0060] Further preferably, the thermal imaging topcoat coating liquid comprises the following raw materials: 15-25 parts of dye dispersion, 30-60 parts of developer dispersion, 10-20 parts of adhesive, 0.5-5 parts of second cross-linking hardener, 0-1.5 parts of defoamer, 0.1-1.5 parts of leveling agent, and 0-1 part of tackifier.
[0061] The dye dispersion and the developer dispersion can be prepared by the method disclosed in the invention patent publication number CN115230360A.
[0062] Preferably, the adhesive is at least one of polyvinyl alcohol, modified polyvinyl alcohol, acrylic latex, styrene-butadiene latex, aliphatic polyurethane emulsion, and polyester resin.
[0063] Preferably, the second cross-linking hardener is at least one of boric acid, borate, aldehyde cross-linking hardener (weight average molecular weight within 120), and polyamide epichlorohydrin.
[0064] Preferably, the defoaming agent is at least one of an acetylenic alcohol defoaming agent, a modified silicone defoaming agent, and a fatty alcohol defoaming agent.
[0065] Preferably, the leveling agent is at least one of a polyether-modified silicone leveling agent, an ethylene oxide-modified silicone leveling agent, a sulfonate leveling agent, and an acetylene alcohol leveling agent.
[0066] Preferably, the thickener is at least one of a polyacrylic acid polymer thickener, a cellulose thickener, alginate, and starch.
[0067] The thermal imaging top coating can be prepared by the method disclosed in the invention patent publication number CN115230360A.
[0068] A fourth aspect of the present invention provides a method for preparing a heat-sensitive recording material.
[0069] A method for preparing a thermal recording material comprises the following steps:
[0070] A thermal imaging topcoat layer is coated on the front side of the substrate, and then the thermal recording material protective liquid is coated on the surface of the thermal imaging topcoat layer, and dried to obtain a protective layer, thereby preparing the thermal recording material.
[0071] Preferably, the drying is hot air drying, and a continuous protective layer is formed after hot air drying.
[0072] Preferably, the coating method is one of extrusion coating, bar coating, blade coating, slit coating, slide coating, and curtain coating. The above coating method is non-direct contact, which is beneficial to controlling the uniformity of the coating. When the protective layer is coated on the surface of the thermal imaging top coating, it is beneficial to the stability of the thermal imaging layer film and avoid interlayer influence or micro-mixing phenomenon, which affects the quality of the printed image.
[0073] More preferably, the coating method is slide coating or curtain coating.
[0074] Preferably, a back coating layer is first applied on the back of the substrate to obtain a back coating layer, a thermal imaging top coating layer is then applied on the front of the substrate, and then a thermal recording material protective liquid is applied on the surface of the thermal imaging top coating layer; or a thermal imaging top coating layer is first applied on the front of the substrate, and then a thermal recording material protective liquid is applied on the surface of the thermal imaging top coating layer, and finally a back coating layer is applied on the back of the substrate.
[0075] A fifth aspect of the present invention provides a use of a heat-sensitive recording material.
[0076] A thermal recording material is used in the fields of printing and medical imaging.
[0077] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0078] The thermal recording material protection liquid provided by the present invention comprises a specific ratio of reactive polyvinyl alcohol, a first cross-linking hardener, an aqueous dispersion of a functional barrier material, a lubricant, a nanofiller, a self-crosslinking reactive latex, and a wetting and leveling agent as main raw materials, wherein the functional barrier material is a modified layered fluorine-containing silicate with a particle size of less than or equal to 100 nm and a stabilizer, and the modified layered fluorine-containing silicate and the stabilizer cooperate with each other to improve the dispersion effect and stability of the thermal recording material protection liquid, and no gel problem occurs. In addition, by adopting the modified layered fluorine-containing silicate, utilizing its layered structure and fluorine-containing characteristics, a good surface barrier effect can be achieved, preventing the transitional precipitation of fusible substances such as lubricants or the shedding of filler debris during high-energy printing, and the friction coefficient is small when in contact with the print head, so that the print head is not worn, and the life of the print head is extended to the greatest extent. Moreover, the modified layered fluorine-containing silicate can be dispersed into a transparent colloidal solution in water, hydrated with water, and form a tighter low-viscosity colloid with the reactive polyvinyl alcohol in the protective liquid, thereby strengthening the cross-linking effect of the reactive polyvinyl alcohol. After coating, a smooth, coherent, stronger and more temperature-resistant film surface is formed on the film surface, making it difficult for the thermal recording material to soften and be damaged during printing, thereby preventing physical scratches or streaks from forming. During the continuous batch printing of images with different printing energies and different printing densities, it can always maintain a good mirror gloss effect, with clear image details and good image quality. In addition, the application of modified layered fluorine-containing silicates can reduce the heavy dependence of the protective layer of heat-sensitive materials on lubricants and fillers (the existing technology, such as the protective layer of Chinese patent CN101247963A, in which the lubricant accounts for 18wt% and the filler accounts for 15-23wt%), avoids the shortcomings of excessive precipitation of lubricants, softening of the protective layer during high-energy printing, easy shedding of filler debris, rough protective layer, precipitation of melt to form sticky heads or debris, etc., and makes it easier to achieve low mutual friction and good lubrication requirements between the protective layer and the print head, while meeting the requirements of high film surface gloss and good image quality when used continuously in large quantities. DETAILED DESCRIPTION
[0079] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0080] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods. In addition, "parts" and "%" in the particles, unless otherwise specified, represent "parts by weight" and "mass percentage" respectively. The particle size of the dispersion was measured using a MASTERSIZER2000 laser particle size analyzer. The viscosity of the dispersion was measured using a Brookfield viscometer.
[0081] Preparation Example 1
[0082] Preparation of functional barrier material aqueous dispersion A: 92 parts of modified lithium magnesium fluorosilicate powder (Bick Chemical, model JS) were slowly added to the stirred water, the stirrer speed was gradually increased to 2500rpm, and 8 parts of tetrasodium pyrophosphate powder were slowly added, mixed and stirred for 0.5h, until it was dispersed into a clear aqueous dispersion with a solid content of 10%. The temperature of the entire preparation process was controlled at 30°C, and the obtained functional barrier material aqueous dispersion A had a test viscosity of 34mpa.s, and could maintain a stable clear aqueous dispersion state within 24h.
[0083] Preparation Example 2 (without adding stabilizer tetrasodium pyrophosphate powder)
[0084] Preparation of functional barrier material aqueous dispersion B: The difference from Preparation Example 1 is that no tetrasodium pyrophosphate powder is added during the preparation process. The obtained functional barrier material aqueous dispersion B has a test viscosity of 42 mpa.s; after standing for 6 hours, it appears in a semi-gel state, and the fluidity becomes poor, and the test viscosity is 144 mpa.s; after standing for 24 hours, it appears in a gel state, and the dispersibility is extremely poor.
[0085] Preparation Example 3 (Replacing Modified Lithium Magnesium Fluorosilicate Powder with Unmodified Lithium Magnesium Silicate Powder)
[0086] Preparation of functional barrier material aqueous dispersion C: 92 parts of lithium magnesium silicate powder (Zhejiang Huate, HectgelRD) were slowly added to the stirred water, the stirrer speed was gradually increased to 2500rpm, and 8 parts of tetrasodium pyrophosphate powder were slowly added, mixed and stirred for 0.5h, until it was dispersed into a clear aqueous dispersion with a solid content of 10%. The temperature of the entire preparation process was controlled at 30°C, and the obtained functional barrier material aqueous dispersion C had a test viscosity of 47mpa.s. After standing for 24h, the fluidity deteriorated and the test viscosity was 164mpa.s.
[0087] Example 1
[0088] A method for preparing a thermal recording material protective liquid comprises the following steps:
[0089] (1) Add 61 parts of KL318 carboxyl-modified polyvinyl alcohol cooking liquid (i.e., carboxyl-modified reactive polyvinyl alcohol, degree of polymerization 2500, Kuraray, Japan) with a mass concentration of 10% into an appropriate amount of clean water, and stir and disperse in a dispersion tank;
[0090] (2) Add 9 parts of aqueous dispersion A of functional barrier material with a solid content of 10% into a dispersion tank and stir for 30 minutes;
[0091] (3) Add 6 parts of lubricant (composed of zinc stearate emulsion F930 and oxidized polyethylene wax emulsion L-548 (Zhongjing Oil), with a composition weight ratio of 1:1), 8 parts of nano silica sol A30 (Grace), 10 parts of polyurethane latex PU-8019 (Yansong Chemical), and 2 parts of wetting and leveling agent DC-67 (Dow Corning) into a dispersion tank in sequence and stir for 20 minutes;
[0092] (4) Add 4 parts of the first cross-linking hardener polyamide epichlorohydrin resin (Japan Starlight, WS4011) into the dispersion tank, add clean water, and stir for 30 minutes to obtain an aqueous protective liquid with a solid content of 8%. The test viscosity is 41 mPa.s.
[0093] Example 2
[0094] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 67 parts of KL318 and 3 parts of functional barrier material aqueous dispersion A are used to obtain a thermal recording material protective liquid with a solid content of 8% and a tested viscosity of 32 mPa.s.
[0095] Example 3
[0096] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 55 parts of KL318 and 15 parts of functional barrier material aqueous dispersion A are used to obtain a thermal recording material protective liquid with a solid content of 8% and a tested viscosity of 55 mPa.s.
[0097] Example 4
[0098] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 67 parts of KL318, 3 parts of a lubricant (composed of zinc stearate emulsion F930 and oxidized polyethylene wax emulsion L-548 (Zhongjing Grease), with a composition mass ratio of 1:1), and 5 parts of nano-silica sol A30 (Grace) are used; a thermal recording material protective liquid with a solid content of 8% is obtained, and a test viscosity of 48 mPa.s is obtained.
[0099] Example 5
[0100] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 57 parts of KL318, 8 parts of a lubricant (composed of zinc stearate emulsion F930 and oxidized polyethylene wax emulsion L-548 (Zhongjing Grease), with a composition weight ratio of 1:1), and 10 parts of nano-silica sol A30 (Grace) are used; an aqueous protective liquid with a solid content of 8% is obtained, and a tested viscosity of 36 mPa.s is obtained.
[0101] Comparative Example 1 (without adding aqueous dispersion of functional barrier material)
[0102] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 70 parts of KL318 and 0 parts of functional barrier material aqueous dispersion A are used to obtain a thermal recording material protective liquid with a solid content of 8% and a tested viscosity of 27 mPa.s.
[0103] Comparative Example 2 (Using Preparation Example 2: Functional barrier material aqueous dispersion B prepared without adding stabilizer tetrasodium pyrophosphate)
[0104] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 9 parts of a functional barrier material aqueous dispersion A with a solid content of 10% are replaced with 9 parts of a functional barrier material aqueous dispersion B with a solid content of 10%; a thermal recording material protective liquid with a solid content of 8% is obtained, and the tested viscosity is 47 mPa.s.
[0105] Comparative Example 3 (Using large particle size filler instead of nano filler)
[0106] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 8 parts of kaolin (average particle size 1 μm) are used to replace the nano-silica sol; an aqueous protective liquid with a solid content of 8% is obtained, and a tested viscosity of 45 mPa.s.
[0107] Comparative Example 4 (Increasing the amount of functional barrier material aqueous dispersion A added)
[0108] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 50 parts of KL318 and 20 parts of functional barrier material aqueous dispersion A are used to obtain a thermal recording material protective liquid with a solid content of 8% and a tested viscosity of 94 mPa.s.
[0109] Comparative Example 5 (reducing the amount of functional barrier material aqueous dispersion A added)
[0110] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 69 parts of KL318 and 1 part of functional barrier material aqueous dispersion A are used to obtain a thermal recording material protective liquid with a solid content of 8% and a tested viscosity of 24 mPa.s.
[0111] Comparative Example 6 (Using Preparation Example 3: Aqueous Dispersion C of Functional Barrier Material Prepared from Lithium Magnesium Silicate Powder)
[0112] A method for preparing a thermal recording material protective liquid, which differs from Example 1 in that 9 parts of a 10% functional barrier material aqueous dispersion A are replaced with 9 parts of a 10% functional barrier material aqueous dispersion C; a thermal recording material protective liquid with a solid content of 8% is obtained, and a tested viscosity of 72 mPa.s.
[0113] Comparative Example 7 (directly adding tetrasodium pyrophosphate powder and modified lithium magnesium fluorosilicate powder without preparing the dispersion in advance)
[0114] A method for preparing a heat-sensitive recording material protective liquid, which is different from Example 1 in that 9 parts of the functional barrier material aqueous dispersion A with a solid content of 10% in step (2) are replaced with 0.9 parts of tetrasodium pyrophosphate powder and modified lithium magnesium fluorosilicate powder (wherein the weight ratio of tetrasodium pyrophosphate powder to modified lithium magnesium fluorosilicate powder is 8:92), and the remaining parts are supplemented with clean water. A heat-sensitive recording material protective liquid with a solid content of 8% is obtained, and the tested viscosity is 24 mPa.s.
[0115] Application Examples 1-5
[0116] The heat-sensitive recording material protective liquid prepared in each example was coated on the surface of the PET film with a back coating on the back and a heat-sensitive imaging top coating on the front by slide coating, with a coating amount of 75 mL / m 2 , dried in a hot air drying oven, and then placed in an environment with a temperature of 50°C and a relative humidity of 50% RH for aging for 16 hours. After the cross-linking and hardening film-forming reaction of the protective layer is fully completed, mature thermal recording materials are obtained.
[0117] Comparative application example 1
[0118] The method of Application Example 1 is adopted, except that the thermal recording material protection liquid of Example 1 is replaced with the thermal recording material protection liquid prepared in Comparative Example 1 to obtain a mature thermal recording material.
[0119] Comparative Application Example 2
[0120] The difference from Comparative Application Example 1 is that the mature thermal recording material is obtained by aging for 48 hours.
[0121] Comparative Application Example 3
[0122] The difference from Comparative Application Example 1 is that the thermal recording material protection liquid of Comparative Example 2 is used to obtain a mature thermal recording material.
[0123] Comparative Application Example 4
[0124] The difference from Comparative Application Example 1 is that the thermal recording material protective liquid of Comparative Example 3 is used to obtain a mature thermal recording material I.
[0125] Comparative Application Example 5
[0126] The difference from Comparative Application Example 1 is that the thermal recording material protection liquid of Comparative Example 4 is used to obtain a mature thermal recording material.
[0127] Comparative Application Example 6
[0128] The difference from Comparative Application Example 1 is that the thermal recording material protection liquid of Comparative Example 5 is used to obtain a mature thermal recording material.
[0129] Comparative Application Example 7
[0130] The difference from Comparative Application Example 1 is that the thermal recording material protection liquid of Comparative Example 6 is used to obtain a mature thermal recording material.
[0131] Comparative Application Example 8
[0132] The difference from Comparative Application Example 1 is that the thermal recording material protection liquid of Comparative Example 7 is used to obtain a mature thermal recording material.
[0133] Product effect testing
[0134] The thermal recording material prepared above was evaluated for high concentration density, surface roughness, surface gloss effect before and after printing, print head sticking, powder falling (debris), surface scratches (black and white scratches), and haze performance. The test method is as follows:
[0135] Density: measured using X-RITE341C (U.S. X-Rite spectrodensitometer).
[0136] Haze: Refer to GB / T2410-2008 "Determination of Transmittance and Haze of Transparent Plastics" and use HT-100 Haze / Transmittance Meter for testing. Low haze indicates good transparency and a clear appearance; high haze indicates poor transparency.
[0137] Surface roughness: refer to GBT 22881-2008 “General method for determination of roughness (smoothness) of paper and paperboard (air leakage method)” and use a PPS surface roughness meter for measurement.
[0138] Use HQ-760DY or HQ-460DY medical thermal imaging printer to continuously print 5,000 sheets of thermal recording materials. After the printer is turned on, the print head will heat up for 2-3 minutes. The printing test can only be started after the print head reaches the required temperature. When printing, the energy of the printing heating point exceeds 100mJ / mm 2, the instantaneous temperature of printing exceeds 170℃, and during printing intervals, the print head maintains a standby temperature of about 60℃. After printing, the following performance evaluation is carried out:
[0139] Surface gloss effect: Every 500 sheets, visually observe the surface of the thermal recording material under reflected light. If the surface is fine and smooth with a mirror-like visual effect, it is "high gloss"; if the surface is rough with a matte visual effect, it is "low gloss". The high-concentration area shows a mirror-like gloss effect. A high gloss indicates that the film formation continuity and high temperature resistance of the protective layer are good. On the contrary, it indicates that the temperature resistance is poor.
[0140] Print head sticking: Use a magnifying glass to observe whether there is molten sticky material or solid sticky material attached to the print head. The less sticky material on the print head surface, the better the effect; otherwise, the effect is poor. The print head sticking effect is graded into "none-mild-medium-severe": "none" means less than 2% of the print head surface has sticky material; "mild" means 2-5% of the print head surface has sticky material; "medium" means 6-10% of the print head surface has sticky material; "severe" means more than 10% of the print head surface has sticky material.
[0141] Powder loss (debris): Every 500 sheets, observe the surface of the thermal recording material after printing to see if there is any white powder or fine debris peeling or falling off during the printing process. The fewer the debris, the better the effect; conversely, the worse the effect. The powder loss (debris) effect is graded into "none-mild-severe": "none" means no powder or debris is observed; "mild" means 1-2 particles of powder or debris can be observed; "severe" means more than 2 particles of powder or debris can be observed.
[0142] Surface scratches: Observe the surface of the thermal recording material after printing every 500 sheets. Under reflected light, check if there are fine scratches in the same printing direction that break the surface of the protective layer, or under transparent light, visually observe if black or white scratches appear on the printed image, destroying the image effect. The fewer scratches, the better the effect; conversely, the worse the effect. The scratch effect is graded into "none-mild-medium-severe": "none" means no scratches or black and white scratches are observed; "mild" means 1-2 scratches can be observed; "medium" means 3-10 scratches can be observed; "severe" means more than 10 scratches can be observed or black and white scratches can be observed.
[0143] The test results are shown in Table 1 below.
[0144] Table 1 Performance test results of the thermosensitive recording materials prepared in each application example and comparative application example
[0145]
[0146] It can be seen from Table 1 that, compared with comparative application examples 1-8, the thermal recording material prepared by using the thermal imaging coating liquid in application example 1-5 has low surface roughness, low haze, high density in the high concentration area, high gloss in the high concentration area, and excellent batch continuous printing performance, without defects such as print head sticking, powder falling, surface scratches, etc., and has excellent image effects. It does not cause negative impact on the continuous use of the printer, avoids the need for excessive manual maintenance of the printing equipment, and is more in line with the needs of large-scale terminal use.
Claims
1. A thermal recording material protective liquid, characterized in that: According to weight parts, it includes the following raw material components: Reactive polyvinyl alcohol 40-90 parts, 1-8 parts of the first cross-linking hardener, 3-18 parts of aqueous dispersion of functional barrier material, 3-8 parts of lubricant, Nano filler 5-10 parts, 5-15 parts of self-crosslinking reaction latex, Wetting and leveling agent 0.5-5 parts; The functional barrier material aqueous dispersion contains modified layered fluorine-containing silicate with a particle size of less than or equal to 100 nm and a stabilizer.
2. The heat-sensitive recording material protective solution according to claim 1, characterized in that: According to weight parts, it includes the following raw material components: Reactive polyvinyl alcohol 50-80 parts, 1-5 parts of the first cross-linking hardener, 3-15 parts of aqueous dispersion of functional barrier material, 3-8 parts of lubricant, Nano filler 5-10 parts, 5-15 parts of self-crosslinking reaction latex, 0.5-2 parts of wetting and leveling agent.
3. The heat-sensitive recording material protective solution according to claim 1, characterized in that: The stabilizer is polyvinyl alcohol and / or pyrophosphate.
4. The heat-sensitive recording material protective solution according to claim 1, characterized in that: The modified layered fluorine-containing silicate is a modified layered fluorine-containing silicate of type S produced by BYK and / or a modified layered fluorine-containing silicate of type JS produced by BYK.
5. The heat-sensitive recording material protective liquid according to claim 1, characterized in that: The reactive polyvinyl alcohol is at least one of carboxyl-modified reactive polyvinyl alcohol, acetoacetyl-modified reactive polyvinyl alcohol, silane-modified reactive polyvinyl alcohol, and diacetone-modified reactive polyvinyl alcohol.
6. The heat-sensitive recording material protective solution according to claim 1, characterized in that: The first cross-linking hardener is at least one of polyamide epichlorohydrin resin, polyaziridine, polycarbodiimide, adipic acid dihydrazide, and aldehyde cross-linking hardener.
7. The method for preparing a heat-sensitive recording material protective liquid according to any one of claims 1 to 6, characterized in that: The steps include: Reactive polyvinyl alcohol and water are mixed and stirred, and an aqueous dispersion of a functional barrier material is added and mixed and stirred. A lubricant, a nanofiller, a self-crosslinking reactive latex, and a wetting and leveling agent are added in sequence and mixed and stirred. A first crosslinking hardener is added to prepare the thermal recording material protective liquid.
8. A thermal recording material, characterized in that: The invention comprises a substrate, a thermal imaging top coating and a protective layer in sequence. The protective layer is obtained by coating the thermal recording material protective liquid according to any one of claims 1 to 6 once. The thermal imaging top coating is coated on the front side of the substrate.
9. The method for preparing a thermal recording material according to claim 8, characterized in that: The steps include: A thermal imaging topcoat layer is coated on the front side of the substrate, and then the thermal recording material protective liquid according to any one of claims 1 to 8 is coated on the surface of the thermal imaging topcoat layer, and dried to obtain a protective layer to prepare the thermal recording material.
10. Use of the thermal recording material according to claim 8 in the fields of printing and medical imaging.
Citation Information
Patent Citations
Transparent thermal recording medium
CN101247963A
Lubricant, preparation method thereof, direct thermal imaging material and preparation method thereof
CN111471508A
Thermo-sensitive imaging coating liquid and application thereof in thermo-sensitive recording material
CN115230360A
Waterproof jet ink plate-making transparent film for print plate-making industry
CN101298216A
Heat-sensitive recording material and method for producing same
CN102341248A
Cited By
Thermal printing material with cleaning function as well as preparation method and application thereof
CN119974800A
Thermal printing material with cleaning function and preparation method and application thereof
CN119974800B
Antistatic, anti-sticking and wear-resistant coating as well as preparation method and application thereof
CN121718219A
Antistatic, anti-adhesive and wear-resistant coating, and method for its production and use
CN121718219B