Waste lithium iron phosphate regeneration lithium supplement agent and preparation method thereof
By preparing lithium-rich lithium ferrite composite materials from waste lithium iron phosphate, using Li5FeO4 core and carbon and lithium phosphide coating layers, the problem of environmental stability and high preparation environment requirements of lithium-rich lithium ferrite was solved, and achieved Cost-effective preparation of electrode materials improves electrochemical performance and stability.
Patent Information
- Application Number
- CN202411198089.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the existing technology, the storage and electrode preparation of lithium-rich lithium ferrite have high environmental requirements, and there are problems such as high residual alkali content, poor environmental stability, and low conductivity, making it difficult to be compatible with the manufacturing process of power batteries.
Using waste lithium iron phosphate to regenerate lithium replenishing agent, through the Li5FeO4 core and the coating layer composed of carbon and lithium phosphide, a cost-effective lithium-rich lithium ferrite (Li5FeO4) composite material is prepared to realize the regeneration of Li, Fe, P, and C elements. Efficient recycling and reuse, reducing the amount of residual alkali and improving electronic conductivity.
It improves the electronic conductivity and air stability of lithium-rich lithium ferrite, reduces the residual alkali content, solves the problems of easy gelation of electrode slurry and large internal resistance of battery polarization, and improves the processability of lithium replenishing agent. and electrochemical properties.
Smart Images

Figure CN118738356A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery recycling and reuse, and in particular to a waste lithium iron phosphate regeneration lithium supplement agent and a preparation method thereof. Background Art
[0002] With the development of new energy vehicles and large-scale energy storage power stations, the output of power batteries and energy storage batteries continues to rise. In the above process, a large number of waste batteries have exerted tremendous pressure on the environment. How to efficiently and economically recycle various elements in battery materials and realize their reuse, thereby building a sustainable development route of green circulation has become a current research hotspot. At present, the mainstream direction is to recycle, regenerate or repair discarded positive electrode materials through technical means such as pyrometallurgy, hydrometallurgy, and direct regeneration, so that they can be reused as low-cost positive electrode materials. However, compared with ternary materials rich in precious metals such as Ni and Co, the economic benefits of recycling lithium iron phosphate are low, and the regenerated lithium iron phosphate material has the problem of poor performance.
[0003] On the other hand, in order to improve the energy storage density of the battery, the installed capacity of new negative electrodes such as silicon-carbon negative electrodes has gradually increased, but this type of negative electrode has a low first coulomb efficiency. In order to form a good solid electrolyte membrane during the first charging of the battery, too much lithium source needs to be consumed, resulting in the loss of the effective capacity of the positive electrode and the decrease of the battery cycle life. Therefore, adding a lithium supplement to the positive electrode has become the current mainstream direction. As a high value-added material, the lithium supplement can irreversibly release the lithium source during the first charging of the battery to supplement the consumption of active lithium by the negative electrode. Among all kinds of lithium supplements, lithium-rich ferrite has the characteristics of high irreversible capacity and has become a current research hotspot, but it has problems such as high residual alkali content, poor environmental stability, and low conductivity, which leads to harsh production environment control of its battery and large battery polarization, limiting large-scale application. CN113603147A proposes a method for preparing lithium-rich ferrite using waste lithium iron phosphate positive electrode material, which prepares high-purity lithium-rich ferrite material by the method of pole piece recovery, pole piece heat treatment, lithium supplement ball milling and roasting. However, this method performs high-temperature air sintering on the pole piece during the heat treatment of the pole piece, resulting in the loss of lithium source and carbon source, and the prepared lithium-rich ferrite does not contain a coating layer, which may have high environmental sensitivity and is difficult to be compatible with the manufacturing process of power batteries. CN116706273A uses hydrofluoric acid to spray-etch the lithium-rich ferrite to construct a lithium fluoride coating layer to reduce the amount of residual alkali and improve the surface structure stability, but hydrofluoric acid is extremely corrosive, which puts great pressure on the corrosion resistance, safety and sewage treatment of production equipment. Therefore, it is urgent to construct a new waste lithium iron phosphate regeneration lithium supplement and its preparation method, so as to efficiently recover and reuse the Li, Fe, P, and C elements in the waste lithium iron phosphate, and solve the current problem of high environmental requirements for the storage and electrode preparation of lithium-rich ferrite. Summary of the invention
[0004] In view of this, the purpose of the present invention is to propose a waste lithium iron phosphate regeneration lithium supplement and its preparation method, so as to solve the current problem of high environmental requirements for the storage and electrode preparation of lithium-rich ferrite, and at the same time solve the problems of easy gelation of electrode slurry and large internal resistance of battery polarization, so as to realize the efficient recovery and reuse of Li, Fe, P and C elements in waste lithium iron phosphate, and prepare cost-effective lithium-rich ferrite (Li 5 FeO 4 ) composite materials.
[0005] Based on the above purpose, the present invention provides a waste lithium iron phosphate regeneration lithium supplement agent, the waste lithium iron phosphate regeneration lithium supplement agent is a lithium-rich lithium iron oxide composite material, which includes Li 5 FeO 4 Core and coating Li 5 FeO 4 The carbon of the inner core and the coating layer composed of lithium phosphide, the molar ratio of Li, Fe and P in the waste lithium iron phosphate regeneration lithium supplement is 5.5~6.3:1:0.5~1, and the carbon content is <5wt%.
[0006] The present invention also provides a method for preparing the waste lithium iron phosphate regeneration lithium supplement agent, comprising the following steps: S1. Recycling of waste lithium iron phosphate materials: first extract the positive electrode of the waste lithium iron phosphate battery, then perform ultrasonic water washing on the positive electrode to separate the electrode powder from the aluminum foil, then filter the separated electrode powder, wash the filter cake with alkali to remove impurities, and wash with deionized water and ethanol until neutral to obtain recycled lithium iron phosphate; among them, there is no special concentration requirement for ethanol, and laboratory alcohol or anhydrous ethanol can be used for washing; S2, preparation of lithium supplementation agent precursor material: firstly, subjecting the recovered lithium iron phosphate to acid leaching and oxidation treatment to chemically remove lithium from the lithium iron phosphate to obtain an iron phosphate solution; then, adding alkali solution to the iron phosphate solution to adjust the pH to 8-10 to cause a precipitation reaction, and after suction filtration and drying, obtaining a mixture material 1 of iron hydroxide and lithium phosphate; finally, subjecting the mixture material 1 to lithium supplementation and dry grinding treatment to obtain a mixture material 2; S3. Preparation of lithium supplement agent: The mixed material 2 is sintered, cooled to room temperature, crushed, and sieved to obtain a lithium supplement agent for regenerating waste lithium iron phosphate.
[0007] Optionally, the method for extracting the positive electrode sheets of the discarded lithium iron phosphate batteries in step S1 is to discharge, disassemble and sort the lithium iron phosphate batteries that have failed in cycles (capacity retention rate <80%) to extract the positive electrode sheets.
[0008] Optionally, the alkali solution used for alkali washing and impurity removal of the filter cake in step S1 includes NaOH solution and / or KOH solution, the concentration of the alkali solution is 0.1-0.5M, and the amount of the alkali solution is 1-3 times the mass of the electrode powder.
[0009] Preferably, the acid solution used for acid leaching in step S2 is a weak acid solution, the weak acid solution includes a phosphoric acid solution, the concentration of the phosphoric acid solution is 0.2-1M, and the amount is based on a P to Fe molar ratio of 1 to 1.05:1; the oxidant used in the oxidation treatment includes hydrogen peroxide, the mass fraction of hydrogen peroxide is 8-30%, and the amount is based on H 2 O 2 The molar ratio to Fe is 1~1.05:1.
[0010] Preferably, deionized water is added during the acid leaching and oxidation treatment in step S2 to adjust the solid content of the solution to 30-45%, the reaction temperature to 40-70° C., and the reaction time to 1-2 hours.
[0011] Preferably, the alkali solution used to adjust the pH in step S2 is aqueous ammonia, the reaction temperature is 40-70° C., and the reaction time is 1-2 hours.
[0012] Optionally, the lithium source used for lithium supplementation in step S2 is one or more of lithium hydroxide, lithium oxide, lithium carbonate, and lithium nitrate, and the added amount is 4-4.5:1 according to the molar ratio of Li to Fe.
[0013] Optionally, the dry grinding device in step S2 is a fusion coating machine or a ball mill; preferably, a fusion coating machine is used, which is conducive to improving the uniform dispersion of the lithium source and the carbon source on the surface of the lithium supplement precursor, thereby improving the sintering efficiency. The inner surface of the fusion coating machine is coated with a tungsten carbide coating, the distance between the blades is 2 mm, the grinding temperature is controlled to be <50°C, the rotation speed is 1000~1500rpm, the grinding time is 30~60 min, and the grinding atmosphere is an inert atmosphere. Inert atmospheres such as nitrogen and argon are sieved through 300 meshes after grinding.
[0014] Optionally, in the sintering process of step S3, the device used is a tube furnace or an atmosphere furnace, the heating rate is 2-5°C / min, the heat treatment temperature is 700-750°C, the holding time is 6-12 hours, and the sintering atmosphere is an inert atmosphere, such as nitrogen and argon.
[0015] Optionally, in the crushing and screening process of step S3, the crushing equipment used is one or more of a jaw crusher, a double-roll crusher, a mechanical crusher, and a jet crusher.
[0016] The recycling of waste lithium iron phosphate materials of the present invention adopts a wet method. After the positive electrode is recycled, the aluminum foil is removed by water washing + alkali washing. No carbon supplement is required, and the carbon source comes from the carbon black in the raw material electrode. Most existing methods adopt a pyrolysis method. After the positive electrode is recycled, it is first subjected to high-temperature treatment. This process will cause the loss of carbon source and lithium source, and carbon supplement is required in the subsequent grinding process.
[0017] Beneficial effects of the present invention: The preparation method of the present invention realizes the efficient recovery and reuse of Li, Fe, P, and C elements in waste lithium iron phosphate, and prepares cost-effective lithium iron-rich lithium (Li 5 FeO 4 ) composite material. The prepared lithium-rich lithium iron oxide composite material has a coating layer composed of carbon and lithium phosphide (C@LixP), which can effectively enhance the electronic conductivity and air stability of lithium-rich lithium iron oxide and reduce the residual alkali content, thereby solving the current problems of short storage time of lithium-rich lithium iron oxide, high requirements for storage and electrode preparation environment, easy gelation of electrode slurry, and large polarization internal resistance of the battery; and improving the processability and electrochemical performance of the lithium supplement. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 The preparation flow chart of the lithium supplement agent for the regeneration of waste lithium iron phosphate; Figure 2 These are the X-ray diffraction characterization results of the regeneration lithium supplement agent for waste lithium iron phosphate. DETAILED DESCRIPTION
[0020] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0021] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by people with ordinary skills in the field to which the present invention belongs. "Include" or "comprising" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, but do not exclude other elements or objects. Example 1
[0022] In this embodiment, the preparation of the waste lithium iron phosphate regeneration lithium supplement agent is carried out according to Figure 1 The specific steps are: S1: Short-circuit and discharge the lithium iron phosphate battery that has failed in the cycle (capacity retention rate <80%), then disassemble it in a low-humidity room and sort out the lithium iron phosphate positive electrode sheets; then, ultrasonically treat the positive electrode sheets in deionized water to separate the electrode powder from the aluminum foil current collector; finally, collect the electrode powder by filtration, and weigh and detect the elements after drying.
[0023] S2: The electrode powder recovered from S1 was placed in a 0.2 M NaOH solution and stirred for 1 hour to remove the metallic aluminum impurities in the powder. The amount of NaOH solution used was 3 times the mass of the positive electrode powder. Subsequently, the powder was filtered and washed alternately with deionized water and ethanol multiple times until the solution was neutral and a filter cake was obtained.
[0024] S3: The filter cake of S2 was placed in a volumetric flask of a condensation recovery device, and 1 M phosphoric acid and 10% mass fraction hydrogen peroxide were added in sequence; wherein, the amount of phosphoric acid added was controlled to control the P / Fe molar ratio to 1.05:1, and the amount of hydrogen peroxide added was controlled to control the H 2 O 2 / Fe molar ratio of 1.05:1; then, deionized water was added to adjust the solid content of the solution to 40%; finally, the solution was stirred at 70°C for 2 hours to allow the lithium iron phosphate to undergo a chemical delithiation reaction to obtain FePO 4 , Li + .
[0025] S4: Add ammonia water to the volumetric flask of S2 and adjust the pH to 9; then, keep the solution temperature at 70°C and age for 2 hours to form Fe(OH) 3 and Li 3 PO 4 finally, filter and wash to obtain the filter cake, which is then dried for later use.
[0026] S5: The filter cake prepared in S4 was placed in a fusion coating machine with a blade spacing of 2 mm, and LiOH powder was added for dry grinding. The amount of LiOH added was controlled to control the Li / Fe molar ratio to 4.5:1. During the grinding process, cooling water was used to control the temperature <50°C, the rotation speed was 1500 rpm, the grinding time was 40 min, and the grinding atmosphere was nitrogen. After grinding, the powder was vibrated and sieved through a 300-mesh screen.
[0027] S6: The powder collected in S5 is placed in a tube furnace for sintering. During the sintering process, nitrogen atmosphere is continuously introduced, the heating rate is 2°C / min, the end temperature is 725°C, and the holding time is 9 hours. After the sintering is completed and cooled to room temperature, the powder is subjected to air flow crushing and sieving to obtain the waste lithium iron phosphate regeneration lithium supplement material (C@LixP@Li 5 FeO 4), its crystal structure is good, and there is no change in diffraction peak after being placed at room temperature and humidity for 24 hours ( Figure 2 ). Example 2
[0028] The only difference between this embodiment and embodiment 1 is that the strong base in step S2 is KOH, and the amount used is 1 times the mass of the positive electrode powder. Example 3
[0029] The difference between this embodiment and embodiment 1 is that the amount of phosphoric acid used in step S3 controls the P / Fe molar ratio to 1:1. Example 4
[0030] The difference between this embodiment and embodiment 1 is that the amount of hydrogen peroxide in step S3 is controlled to be 2 O 2 / Fe molar ratio 1:1. Example 5
[0031] The only difference between this embodiment and embodiment 1 is that the solid content of the solution in step S3 is 30%, the reaction temperature is 40° C., and the reaction time is 1 hour. Example 6
[0032] The only difference between this embodiment and embodiment 1 is that the pH in step S4 is controlled to be 10 and the aging time is 1 hour. Example 7
[0033] The only difference between this embodiment and embodiment 1 is that the lithium source in step S5 is lithium carbonate, and the amount added is controlled to have a Li / Fe molar ratio of 4:1. Example 8
[0034] The only difference between this embodiment and embodiment 1 is that the lithium source in step S5 is lithium nitrate, and the added amount is controlled to have a Li / Fe molar ratio of 4:1. Example 9
[0035] The only difference between this embodiment and embodiment 1 is that the grinding time in step S5 is 30 min. Example 10
[0036] The only difference between this embodiment and embodiment 1 is that the grinding time in step S5 is 60 min. Embodiment 11
[0037] The only difference between this embodiment and embodiment 1 is that the sintering temperature in step S6 is 700° C. and the sintering time is 12 hours. Example 12
[0038] The only difference between this embodiment and embodiment 1 is that the sintering temperature in step S6 is 750° C. and the sintering time is 6 hours.
[0039] Comparative Example 1 The difference between this comparative example and Example 1 is that there is no step S2 and no strong alkali washing is used to remove aluminum impurities in the electrode powder.
[0040] Comparative Example 2 The difference between this comparative example and Example 1 is that in step S3, the reaction temperature is room temperature (20° C.) and the reaction time is 6 hours.
[0041] Comparative Example 3 The difference between this comparative example and Example 1 is that in step S4, the reaction temperature is room temperature (20° C.) and the reaction time is 6 hours.
[0042] Comparative Example 4 The difference between this comparative example and Example 1 is that in step S4, the pH is adjusted to 7.
[0043] Comparative Example 5 The only difference between this comparative example and Example 1 is that in step S6, the sintering temperature is 800°C.
[0044] The waste lithium iron phosphate regeneration and lithium supplement agent obtained in the above examples and comparative examples was used to prepare a positive electrode for a lithium-ion battery, and an electrochemical performance test was performed. The specific method includes mixing the composite material, conductive carbon black, and PVDF in NMP at a mass ratio of 80:10:10. After coating, baking, and rolling, a positive electrode for a lithium-ion battery was prepared. A commercial lithium-ion battery electrolyte (1M LiPF 6 In EC / DMC (vol. 1:1)) button cells were assembled and constant current charge and discharge tests were performed. The electrode was metallic lithium and the separator was Celgard 2400. The test results are shown in Table 1.
[0045]
[0046] Examples 1 and 2 illustrate that changing the type of strong alkali in the alkaline washing process and reducing the washing time can effectively remove aluminum impurities in the raw materials, and the prepared lithium supplement has a high first charge capacity. Comparative Example 1 shows that without using a strong alkali to remove aluminum impurities in the waste lithium iron phosphate raw materials, the prepared lithium supplement has more impurities and a low first charge capacity. Examples 1, 3, and 4 show that reducing the amount of phosphoric acid and oxidant used in the acid leaching process slightly reduces the first charge capacity of the prepared lithium supplement. Examples 1 and 5 illustrate that under controlled conditions, reducing the temperature, solid content and reaction time, the prepared lithium supplement can still provide a high first charge capacity and have a low coulomb efficiency. Comparative Example 2 illustrates that reducing the reaction temperature in the acid leaching process to room temperature (20°C), even if the reaction time is increased to 6 hours, the leaching efficiency of lithium iron phosphate is low, and the prepared lithium supplement has a lithium iron phosphate impurity phase, a low first charge capacity, and a high coulomb efficiency. Examples 1, 6 and Comparative Example 4 illustrate that in the precipitation process, when the pH value is adjusted to a low level (7), it is difficult for the precursor to form Fe(OH) 3 and Li 3 PO 4 , the prepared lithium supplement has a lithium iron phosphate phase, the first charge capacity is low and the coulomb efficiency is high. Similarly, Example 3 shows that by lowering the temperature in the precipitation process and extending the reaction time, the first charge capacity of the prepared lithium supplement is greatly reduced. Examples 1 and 8 show that changing the type of lithium salt in dry grinding can also prepare a lithium supplement with a high irreversible capacity. Examples 1, 9, and 10 show that increasing the dry grinding time can improve the uniformity of the reaction and increase the first charge capacity of the prepared lithium supplement. Examples 1, 11, and 12 show that by controlling the sintering temperature in the range of 700~750°C, the prepared lithium supplement has a good phase and has a high first charge capacity. Comparative Example 5 shows that increasing the sintering temperature to 800°C will enhance the reducibility of the residual carbon in the raw materials, thereby destroying the structure of the lithium supplement and causing a significant reduction in the first charge capacity.
[0047] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A waste lithium iron phosphate regeneration lithium supplement agent, characterized in that: The waste lithium iron phosphate regeneration lithium supplement agent is a lithium-rich lithium iron oxide composite material, which includes a Li5FeO4 core and a coating layer composed of carbon and lithium phosphide coating the Li5FeO4 core. The molar ratio of Li, Fe and P in the waste lithium iron phosphate regeneration lithium supplement agent is 5.5~6.3:1:0.5~1, and the carbon content is <5wt%.
2. A method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 1, characterized in that: The steps include: S1. Recovery of waste lithium iron phosphate materials: first extract the positive electrode sheets of the waste lithium iron phosphate batteries, then perform ultrasonic water washing on the positive electrode sheets to separate the electrode powder from the aluminum foil, then filter the separated electrode powder, wash the filter cake with alkali to remove impurities, and wash with deionized water and ethanol alternately until neutral to obtain recovered lithium iron phosphate; S2. Preparation of precursor materials for lithium supplementing agent: firstly, subjecting the recovered lithium iron phosphate to acid leaching and oxidation treatment to cause the lithium iron phosphate to undergo chemical delithiation reaction to obtain an iron phosphate solution; Then, an alkali solution is added to the ferric phosphate solution to adjust the pH to 8-10, so that a precipitation reaction occurs, and after suction filtration and drying, a mixture material 1 of ferric hydroxide and lithium phosphate is obtained; finally, the mixture material 1 is subjected to lithium supplementation and dry grinding treatment to obtain a mixture material 2; S3. Preparation of lithium supplement agent: The mixed material 2 is sintered, cooled to room temperature, crushed, and sieved to obtain a lithium supplement agent for regenerating waste lithium iron phosphate.
3. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: The alkali solution used for alkali washing and impurity removal of the filter cake in step S1 includes NaOH solution and / or KOH solution, the concentration of the alkali solution is 0.1-0.5M, and the amount of the alkali solution is 1-3 times the mass of the electrode powder.
4. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: The acid solution used for acid leaching in step S2 is a weak acid solution, which includes a phosphoric acid solution, the concentration of the phosphoric acid solution is 0.2-1M, and the molar ratio of P to Fe is 1-1.05:1; the oxidant used in the oxidation treatment includes hydrogen peroxide, the mass fraction of hydrogen peroxide is 8-30%, and the molar ratio of H2O2 to Fe is 1-1.05:
1.
5. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: In step S2, deionized water is also added during the acid leaching and oxidation treatment to adjust the solid content of the solution to 30-45%, the reaction temperature to 40-70° C., and the reaction time to 1-2 hours.
6. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: The alkali solution used to adjust the pH in step S2 is ammonia water, the reaction temperature is 40-70° C., and the reaction time is 1-2 hours.
7. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: The lithium source used for lithium supplementation in step S2 is one or more of lithium hydroxide, lithium oxide, lithium carbonate, and lithium nitrate, and the added amount is based on a molar ratio of Li to Fe of 4 to 4.5:
1.
8. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: The device for dry grinding in step S2 is a fusion coating machine or a ball mill; when a fusion coating machine is used, the inner cavity surface is coated with a tungsten carbide coating, the blade spacing is 2 mm, the grinding temperature is controlled to be <50°C, the rotation speed is 1000~1500 rpm, the grinding time is 30~60 min, and the grinding atmosphere is an inert atmosphere.
9. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: In the sintering process of step S3, the device used is a tubular furnace or an atmosphere furnace, the heating rate is 2-5°C / min, the heat treatment temperature is 700-750°C, the holding time is 6-12 hours, and the sintering atmosphere is an inert atmosphere.
10. The method for preparing the waste lithium iron phosphate regeneration lithium supplement agent according to claim 2, characterized in that: In the crushing and screening process of step S3, the crushing equipment used is one or more of a jaw crusher, a double-roll crusher, a mechanical crusher, and a jet crusher.
Citation Information
Patent Citations
Method for preparing pre-lithiation agent by using waste lithium iron phosphate positive electrode material
CN113603147A
Lithium-supplementing additive for lithium-rich lithium ferrite positive electrode, preparation method of lithium-supplementing additive and lithium ion battery positive electrode
CN116706273A
Method for preparing lithium battery electrode materials LiFePO4 and Li4Ti5O12 from vanadium extraction slag
CN104805299A
Method for preparing phosphorus-doped lithium-rich lithium ferrite from waste lithium iron phosphate pole pieces and obtained product
CN116315218A
Lithium-rich composite material and preparation method and application thereof
CN117293317A
Cited By
Lithium supplement additive Li5FeO4 and preparation method thereof
CN120398125A
A lithium supplement additive, Li5FeO4, and its preparation method
CN120398125B
Lithium-replenishing agent and preparation method therefor, positive electrode sheet and secondary battery
WO2026143716A1