Preparation method and application of 1D HKUST-1 / PEO-based solid electrolyte membrane

By uniformly distributing 1D HKUST-1 in the PEO-based solid electrolyte, a one-dimensional continuous pore structure is formed, which solves the problems of low conductivity and insufficient mechanical strength of the PEO-based electrolyte, significantly improves the lithium ion conductivity and cycle stability, and improves performance of lithium metal batteries.

CN118738538APending Publication Date: 2024-10-01ANHUI LEOCH PENEWABLE ENERGY DEV CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410633345.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The PEO-based solid electrolyte has small room temperature conductivity, poor mechanical strength and low electrochemical window, which cannot meet the needs of a wide range of uses, and fillers such as MOF structures are difficult to effectively guide the formation of continuous lithium ion transport paths at high concentrations.

Method used

Using the preparation method of 1D HKUST-1/PEO-based solid electrolyte membrane, activated 1D HKUST-1 is formed by self-assembly of modified cellulose with copper nitrate trihydrate and 1,3,5-benzenetricarboxylic acid in methanol. Ultrasonic treatment is evenly distributed in PEO to form a one-dimensional continuous pore structure, which regulates the Lewis acid-base interaction in the system and enhances lithium ion migration.

Benefits of technology

Significantly improves lithium ion conductivity and cycle stability, improves lithium dendrite growth and interface stability, and improves the charge and discharge performance and stability of lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738538A_ABST
    Figure CN118738538A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a 1DHKUST-1 / PEO-based solid electrolyte membrane, and relates to the technical field of lithium metal batteries. The preparation method comprises the following steps: S1, preparing modified cellulose; s2, preparing the 1DHKUST-1; s3, preparing a solid electrolyte membrane; cellulose is modified, HKUST-1 particles are densely and orderly arranged on fibers of the modified long-strip-shaped cellulose, and a one-dimensional continuous pore structure is formed; uniform dispersion sites and clear channels are provided for ion diffusion, uniform deposition of lithium ions in the charging and discharging process is promoted, the stability of an interface is promoted, and the problem of lithium dendrite growth is solved; the HKUST-1 has a specific periodic high-porosity structure, contains highly dispersed metal active sites and C = O sites, shows a selective adsorption result on TFSI-, and can capture TFSI-to improve the lithium ion transference number and improve the lithium ion conductivity of the polymer electrolyte membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium metal batteries, and in particular to a preparation method and application of a 1D HKUST-1 / PEO-based solid electrolyte membrane. Background Art

[0002] Solid electrolytes are the core of solid-state lithium metal batteries. They isolate the positive and negative electrodes, prevent short circuits, and conduct ions. They largely determine the performance parameters of solid-state lithium metal batteries, such as power density, cycle stability, high and low temperature performance, etc. Solid electrolytes can be divided into inorganic solid electrolytes, organic solid electrolytes, and composite solid electrolytes. The performance of different types of electrolytes varies greatly. Among them, organic polymer solid electrolytes have good flexibility, simple preparation process, and good interface compatibility with electrodes.

[0003] PEO is the most studied polymer solid electrolyte, but its relatively small room temperature conductivity (10 -7 ~10 -5 S cm -1 ), poor mechanical strength, and low electrochemical window, which cannot meet the needs of a wide range of uses. In order to solve these problems, solid plasticizers, ceramic particles and other fillers are usually added or copolymerized with other polymer monomers to improve the mechanical properties of the material and the stability with lithium metal, and effectively improve the conductivity of the polymer electrolyte. Modification by filler is a simple and low-cost modification method. Fillers are mostly inorganic lithium ion conductor materials, inert oxides that do not contain lithium ions, metal organic frameworks, etc. The MOF structure is a type of crystalline porous material with a periodic network structure formed by the self-assembly of inorganic metal centers (metal ions or metal clusters) and bridging organic ligands. It has a unique structure and contains metal centers, and is often used as a lithium battery electrolyte additive to improve the electrochemical performance of lithium batteries. However, these fillers tend to aggregate at relatively high concentrations, making it difficult to effectively guide the formation of continuous lithium ion transmission paths. Summary of the invention

[0004] In order to solve at least one of the above technical problems and develop a PEO-based polymer solid electrolyte with high ionic conductivity, the present application provides a preparation method and application of a 1D HKUST-1 / PEO-based solid electrolyte membrane.

[0005] On the one hand, the present application provides a method for preparing a 1D HKUST-1 / PEO-based solid electrolyte membrane, comprising the following steps:

[0006] S1 Preparation of modified cellulose

[0007] Adding microcrystalline cellulose powder and 3-aminopropyltrimethoxysilane to deionized water, stirring at room temperature, and collecting the product by centrifugation; adding the product and sodium polystyrene sulfonate aqueous solution to deionized water, ultrasonically dispersing, and centrifuging to obtain modified cellulose;

[0008] S2 Preparation of 1D HKUST-1

[0009] The modified cellulose prepared in S1, copper nitrate trihydrate, and 1,3,5-benzenetricarboxylic acid were added to methanol, stirred at room temperature, and centrifuged to obtain a preliminary product, which was freeze-dried and activated to obtain activated 1D HKUST-1;

[0010] S3 Preparation of solid electrolyte membrane

[0011] 1D HKUST-1 and LiTFSI were weighed separately and added to acetonitrile, ultrasonically mixed, PEO was added, stirred to form a viscous liquid, introduced into a mold, dried and allowed to stand to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane.

[0012] Optionally, in S1, the content of sodium polystyrene sulfonate in the sodium polystyrene sulfonate aqueous solution is 30wt%; the ratio of the added amounts of the microcrystalline cellulose powder, 3-aminopropyltrimethoxysilane and the sodium polystyrene sulfonate aqueous solution is: for every 170mg of microcrystalline cellulose powder, the added amount of 3-aminopropyltrimethoxysilane is 3ml, and the added amount of the sodium polystyrene sulfonate aqueous solution is 6ml.

[0013] Optionally, in S1, the ultrasonic dispersion time is 1 h.

[0014] Optionally, in S2, the molar ratio of the copper nitrate trihydrate to 1,3,5-benzenetricarboxylic acid is 1:4.

[0015] Optionally, in S2, the stirring time at room temperature is 3 h.

[0016] Optionally, in S3, the addition amount of 1D HKUST-1 relative to PEO is 1 wt% to 5 wt%.

[0017] Optionally, in S3, the addition amount of 1D HKUST-1 relative to PEO is 3 wt%.

[0018] Optionally, in S3, the ultrasonic mixing time is 1 hour.

[0019] Optionally, in S3, the drying standing time is 3 days.

[0020] In a second aspect, the present application also provides the use of a 1DHKUST-1 / PEO-based solid electrolyte membrane prepared by the above-mentioned preparation method in a lithium metal battery.

[0021] In summary, the present application includes at least one of the following beneficial technical effects:

[0022] 1. The high specific surface area of ​​HKUST-1 facilitates full contact with the PEO solid electrolyte. Its surface polarity can regulate the interaction between Lewis acid and base in the system and optimize the electrochemical performance of SSE. HKUST-1 has a specific periodic high-porosity structure, contains highly dispersed metal active sites and C=O sites, and exhibits selective adsorption results for TFSI-, which can capture TFSI - Improve the lithium ion migration number and the lithium ion conductivity of the polymer electrolyte membrane;

[0023] 2. By modifying cellulose, HKUST-1 particles are densely and orderly arranged on the modified long strips of cellulose fibers, forming a one-dimensional continuous pore structure; providing uniformly dispersed sites and clear channels for ion diffusion, promoting uniform deposition of lithium ions during charge and discharge, promoting interface stability, and improving the problem of lithium dendrite growth;

[0024] 3. The charge and discharge performance of the lithium metal battery assembled with the PEO-based solid electrolyte membrane with 1D HKUST-1 can be significantly improved; and the performance of the lithium metal battery is very stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the 1D HKUST-1 prepared in the preparation example of this application;

[0026] Figure 2 This is a temperature impedance relationship test diagram of the 1D HKUST-1 / PEO-based solid electrolyte membrane prepared in Examples 1 to 3 of the present application;

[0027] Figure 3 This is a cycle performance diagram of the lithium metal battery assembled corresponding to Example 2 of the present application. DETAILED DESCRIPTION

[0028] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0029] This application designs a method for preparing a 1D HKUST-1 / PEO-based solid electrolyte membrane, comprising the following steps:

[0030] S1 Preparation of modified cellulose

[0031] Adding microcrystalline cellulose powder and 3-aminopropyltrimethoxysilane to deionized water, stirring at room temperature, and collecting the product by centrifugation; adding the product and sodium polystyrene sulfonate aqueous solution to deionized water, ultrasonically dispersing, and centrifuging to obtain modified cellulose;

[0032] S2 Preparation of 1D HKUST-1

[0033] The modified cellulose prepared in S1, copper nitrate trihydrate, and 1,3,5-benzenetricarboxylic acid were added to methanol, stirred at room temperature, and centrifuged to obtain a preliminary product, which was freeze-dried and activated to obtain activated 1D HKUST-1;

[0034] S3 Preparation of solid electrolyte membrane

[0035] 1D HKUST-1 and LiTFSI were weighed separately and added to acetonitrile, ultrasonically mixed, PEO was added, stirred to form a viscous liquid, introduced into a mold, dried and allowed to stand to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane.

[0036] The surface polarity of HKUST-1 can regulate the Lewis acid-base interaction in the system and optimize the electrochemical performance of PEO-based solid electrolytes; HKUST-1 has a specific periodic high-porosity structure, which provides uniformly dispersed sites and clear migration channels for Li+; HKUST-1 contains highly dispersed metal active sites and C=O sites, which can synergistically adsorb TFSI - , which is beneficial to increase the number of lithium ion migration.

[0037] However, simply adding HKUST-1 to the PEO-based solid electrolyte does not achieve good results due to the aggregation of HKUST-1. Therefore, the inventors have developed the technical solution of the present application, in which cellulose is modified once by 3-aminopropyltrimethoxysilane and sodium polystyrene sulfonate aqueous solution, and organic ligands and metal salts are used as raw materials. Through liquid phase reaction, HKUST-1 particles are densely and orderly arranged on the long strips of modified cellulose fibers to obtain a metal organic framework (1DHKUST-1) with a specific one-dimensional continuous pore structure and highly dispersed metal active sites and C=O sites. Then, through ultrasonic treatment, 1D HKUST-1 is evenly distributed in the PEO-based solid electrolyte, thereby effectively reducing the aggregation of HKUST-1 particles.

[0038] By evenly distributing 1D HKUST-1 in the solid electrolyte membrane, a continuous and rapid transmission path is provided for lithium ions, which can improve the lithium ion conductivity of the solid electrolyte membrane. The ordered arrangement structure and high dispersion of 1DHKUST-1 help the uniform deposition of lithium ions, promote the stability of the interface, and solve the problem of lithium dendrite growth. The ionic conductivity and cycle stability of the solid electrolyte membrane prepared by this application have been significantly improved.

[0039] In the following examples of the present application, the main components involved, unless otherwise specified, were purchased from commercially available products.

[0040] Microcrystalline cellulose powder, particle size is 10nm~200nm. Specific embodiments

[0042] Preparation Example

[0043] This preparation example is used to prepare a one-dimensional ordered metal-organic framework (1D HKUST-1).

[0044] 170 mg of microcrystalline cellulose powder and 3 mL of 3-aminopropyltrimethoxysilane were added to 200 mL of deionized water and stirred at room temperature for 18 hours; the dispersion was then centrifuged to collect the product. The above product and 6 mL of a 30 wt% sodium polystyrene sulfonate aqueous solution were added to 300 mL of deionized water and ultrasonically dispersed for 1 hour; the dispersion was then centrifuged to obtain modified cellulose.

[0045] The modified cellulose collected above, 1208 mg (5 mmol) of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 4202 mg (20 mmol) of 1,3,5-benzenetricarboxylic acid were added to 150 mL of methanol and stirred at room temperature for 3 h; the dispersion was then separated by centrifugation to obtain 1D HKUST-1, and the activated 1D HKUST-1 was obtained by freeze-drying.

[0046] like Figure 1 The SEM image of 1D HKUST-1 prepared in this preparation example is shown in FIG.

[0047] HKUST-1 particles are densely and orderly arranged on the long strips of modified cellulose fibers, forming a one-dimensional continuous pore structure.

[0048] Examples 1 to 3 are used to prepare 1D HKUST-1 / PEO-based solid electrolyte membranes.

[0049] Example 1

[0050] In the glove box, 4.4 mg of 1D HKUST-1 prepared in the preparation example and 179.4 mg of LiTFSI were weighed and added to a weighing bottle containing 7 mL of acetonitrile, and ultrasonically mixed for 1 h to uniformly disperse 1D HKUST-1 in the solution; then 440 mg of PEO particle powder was added to the above weighing bottle and stirred to form a uniform viscous liquid. The solution was then introduced into a polytetrafluoroethylene mold and left to dry in the glove box for 3 days to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane (PEO+1wt%1D HKUST-1).

[0051] Example 2

[0052] In the glove box, 13.2 mg of 1D HKUST-1 prepared in the preparation example and 179.4 mg of LiTFSI were weighed and added to a weighing bottle containing 7 mL of acetonitrile, and ultrasonically mixed for 1 h to make 1D HKUST-1 evenly dispersed in the solution; then 440 mg of PEO particle powder was added to the above weighing bottle and stirred to form a uniform viscous liquid. The solution was then introduced into a polytetrafluoroethylene mold and left to dry in the glove box for 3 days to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane (PEO+3wt%1D HKUST-1).

[0053] Example 3

[0054] In the glove box, 22 mg of 1D HKUST-1 prepared in the preparation example and 179.4 mg of LiTFSI were weighed and added to a weighing bottle containing 7 mL of acetonitrile, and ultrasonically mixed for 1 h to make 1D HKUST-1 evenly dispersed in the solution; then 440 mg of PEO particle powder was added to the above weighing bottle and stirred to form a uniform viscous liquid. The solution was then introduced into a polytetrafluoroethylene mold and left to dry in the glove box for 3 days to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane (PEO+5wt%1DHKUST-1).

[0055] The temperature impedance relationship of the 1D HKUST-1 / PEO-based solid electrolyte membrane prepared in Examples 1 to 3 was tested. The results are as follows: Figure 2 shown.

[0056] pass Figure 2It can be seen that the performance of the solid electrolyte membrane prepared in Example 2 of the present application with the addition of 3wt% 1D HKUST-1 is slightly better than that of the solid electrolyte membrane prepared in Example 1 with the addition of 1wt% 1D HKUST-1, and the performance of the solid electrolyte membrane in Example 3 obtained by continuing to increase 1D HKUST-1 to 5wt% is significantly decreased; however, the performance of the solid electrolyte membrane with the addition of 1D HKUST-1 at 1wt% to 5wt% is significantly better than that of the PEO-based solid electrolyte membrane without the addition of 1D HKUST-1.

[0057] The 1D HKUST-1 / PEO-based solid electrolyte membrane prepared in Example 2 was assembled into a lithium metal battery, and the specific process was as follows.

[0058] The 1D HKUST-1 / PEO-based solid electrolyte membrane was cut in a glove box, and then the CR2032 button battery was assembled in the order of positive electrode shell, positive electrode, solid electrolyte membrane, lithium metal negative electrode, gasket, spring and negative electrode shell.

[0059] The electrochemical impedance spectrum of the button cell assembled above was tested using an Autolab electrochemical workstation and a constant temperature and humidity chamber at 25-70°C. The charge and discharge performance of the button cell assembled above was tested using a LandCT3002A battery testing system at room temperature. The cycle performance of the lithium metal battery obtained by the test is shown in the figure below. Figure 3 shown.

[0060] The performance of the lithium metal battery assembled with the PEO-based solid electrolyte membrane prepared in Example 2 with 3 wt% 1D HKUST-1 is significantly better than that of the lithium metal battery assembled with the PEO-based solid electrolyte membrane without 1D HKUST-1. In addition, the performance of the lithium metal battery assembled with the solid electrolyte membrane in Example 2 of the present application is very stable.

[0061] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a 1D HKUST-1 / PEO-based solid electrolyte membrane, characterized in that: The following steps are involved: S1 Preparation of modified cellulose Adding microcrystalline cellulose powder and 3-aminopropyltrimethoxysilane to deionized water, stirring at room temperature, and collecting the product by centrifugation; adding the product and sodium polystyrene sulfonate aqueous solution to deionized water, ultrasonically dispersing, and centrifuging to obtain modified cellulose; S2 Preparation of 1D HKUST-1 The modified cellulose prepared in S1, copper nitrate trihydrate, and 1,3,5-benzenetricarboxylic acid were added to methanol, stirred at room temperature, and centrifuged to obtain a preliminary product, which was freeze-dried and activated to obtain activated 1D HKUST-1; S3 Preparation of solid electrolyte membrane 1D HKUST-1 and LiTFSI were weighed separately and added to acetonitrile, ultrasonically mixed, PEO was added, stirred to form a viscous liquid, introduced into a mold, dried and allowed to stand to obtain a 1D HKUST-1 / PEO-based solid electrolyte membrane.

2. The preparation method according to claim 1, characterized in that: In S1, the content of sodium polystyrene sulfonate in the sodium polystyrene sulfonate aqueous solution is 30wt%; the ratio of the added amounts of the microcrystalline cellulose powder, 3-aminopropyltrimethoxysilane and the sodium polystyrene sulfonate aqueous solution is: for every 170mg of microcrystalline cellulose powder, the added amount of 3-aminopropyltrimethoxysilane is 3ml, and the added amount of the sodium polystyrene sulfonate aqueous solution is 6ml.

3. The preparation method according to claim 1, characterized in that: In S1, the ultrasonic dispersion time is 1 h.

4. The preparation method according to claim 1, characterized in that: In S2, the molar ratio of the copper nitrate trihydrate to 1,3,5-benzenetricarboxylic acid is 1:

4.

5. The preparation method according to claim 1, characterized in that: In S2, the stirring time at room temperature is 3 h.

6. The preparation method according to claim 1, characterized in that: In the S3, the addition amount of 1DHKUST-1 relative to PEO is 1 wt% to 5 wt%.

7. The preparation method according to claim 6, characterized in that: In S3, the addition amount of 1DHKUST-1 relative to PEO is 3 wt %.

8. The preparation method according to claim 1, characterized in that: In S3, the ultrasonic mixing time is 1 h.

9. The preparation method according to claim 1, characterized in that: In S3, the drying standing time is 3 days.

10. Use of the 1D HKUST-1 / PEO-based solid electrolyte membrane prepared in claim 1 in a lithium metal battery.

Citation Information

Cited By

  • HKUST-1 (at) CNF composite material as well as preparation method and application thereof

    CN119306956A

  • Gas sensor based on metal organic framework and cellulose and preparation method

    CN121410080A