Urea plasticized thermoplastic chitosan adsorption film and melting processing method thereof

Through urea plasticization technology, the problem of low mechanical properties and reduced adsorption effect caused by excessive plasticizer content in thermoplastic chitosan film materials has been solved, and the thermoplastic processing and excellent adsorption performance of high-content chitosan have been achieved.

CN118767894APending Publication Date: 2024-10-15HUBEI UNIV OF EDUCATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410639684.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the preparation of existing thermoplastic chitosan film materials, the plasticizer content is too high, resulting in low mechanical properties, and the use of a large amount of additives reduces the adsorption effect of chitosan.

Method used

Urea is used as a plasticizer, mixed evenly with chitosan and dilute hydrochloric acid solution, and then melted and processed in an internal mixer. The process conditions are controlled to improve the thermoplastic processability and adsorption performance of chitosan and ensure the solid content of chitosan. above 50%.

Benefits of technology

The flexibility and adsorption properties of chitosan are improved, the efficient metal ion adsorption effect is maintained, and the mechanical properties of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767894A_ABST
    Figure CN118767894A_ABST
Patent Text Reader

Abstract

The invention discloses a urea plasticized thermoplastic chitosan adsorption film and a melting processing method thereof. The invention relates to the technical field of chitosan materials. The preparation method comprises the following steps: uniformly mixing chitosan, urea and a solvent, pouring the mixture into an internal mixer, mixing to obtain thermoplastic chitosan, and carrying out hot pressing on the thermoplastic chitosan to obtain the thermoplastic chitosan film. Due to the addition of the urea, not only can the thermoplastic processability of the chitosan be improved, but also the flexibility of the thermoplastic chitosan material can be improved, and urea molecules can reduce the hydrogen-bond interaction between the chitosan and promote the thermoplastic processability of the chitosan; in the processing process, urea small molecules permeate into a chitosan molecular chain, so that the motility of the chitosan molecular chain is improved, and the flexibility of chitosan is improved. Meanwhile, a net structure formed by the urea and the chitosan due to hydrogen bonds and amino groups on urea molecules play a synergistic role in metal ion adsorption, and the problems that the adsorption performance of the chitosan is reduced due to the fact that the content of the chitosan is reduced and the like are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chitosan materials, in particular to a urea plasticized thermoplastic chitosan adsorption film and a melting processing method thereof. Background Art

[0002] Chitosan is known as "animal cellulose" and is the only cationic alkaline polysaccharide that exists in large quantities in nature. It is non-toxic, has good film-forming properties, is biocompatible, biodegradable, and is not prone to secondary pollution. The excellent properties of chitosan make it have potential application value in agriculture, food, medicine, and environmental protection. The chitosan molecular chain contains abundant active groups such as -OH and -NH2, which can form cage-shaped molecules with a similar network structure through hydrogen bonds and ionic bonds, so that chitosan can combine with almost all transition metal ions, has a stable coordination effect on heavy metal ions, and can form complexes with metals, and has a good adsorption effect on heavy metal ions.

[0003] There are two main methods for preparing chitosan adsorption film materials: solution method and thermoplastic processing method. The solution method requires the use of a large amount of solvent, and in the process of post-processing, the performance of the film is greatly affected by the drying temperature and time, which reduces the controllability of the preparation and is not conducive to the large-scale production of the film. Thermoplastic processing is to heat the material to "melt", mix and modify it in the processing equipment, and then directly process it into a film in the hot pressing equipment. This method is simple and is an ideal method for material processing and production. Similar to other natural polymers, chitosan itself has no melting point and cannot be directly heated and melted. Therefore, the thermoplastic processing of chitosan needs to be carried out under the action of plasticizers. However, there are two problems in the preparation of thermoplastic chitosan film materials: one is that the content of the added plasticizer is too high (70-80%), and the mechanical properties of the obtained chitosan material are very low and not practical. Second, the use of a large number of additives reduces the content of chitosan itself and affects its adsorption effect. Summary of the invention

[0004] The object of the present invention is to provide a urea plasticized thermoplastic chitosan adsorption film and a melt processing method thereof in view of the above-mentioned deficiencies in the prior art.

[0005] The invention discloses a melt processing method for a urea plasticized thermoplastic chitosan adsorption film. Chitosan, urea and a solvent are uniformly mixed and poured into an internal mixer for mixing to obtain thermoplastic chitosan.

[0006] Furthermore, the solvent includes one or more of dilute hydrochloric acid, acetic acid, and lactic acid.

[0007] Furthermore, when the acid solution is dilute hydrochloric acid, the mass fraction of the dilute hydrochloric acid is 5% to 8%.

[0008] Furthermore, the mass ratio of chitosan to dilute hydrochloric acid is 1:1.5.

[0009] Furthermore, the urea accounts for 5% to 20% of the sum of the mass of chitosan and urea.

[0010] Furthermore, the banburying temperature is 60-90° C. and the banburying time is 5-15 min.

[0011] Furthermore, the deacetylation degree of the chitosan is greater than 85%.

[0012] Furthermore, the weight average molecular weight of the chitosan is 50,000 to 200,000.

[0013] A urea plasticized thermoplastic chitosan adsorption film prepared by the above-mentioned preparation method.

[0014] The urea plasticized thermoplastic chitosan adsorption film has a solid content of chitosan of more than 50% and is used for adsorbing heavy metal ions.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] When acid solution, urea and chitosan are mixed in a certain proportion, the H + The amino groups on urea can react with the amino and hydroxyl groups on the chitosan molecules, reduce the interaction between the chitosan molecular chains themselves, increase the mobility of the chitosan molecular chains, and reduce the melting point of chitosan, so that it can melt before the decomposition temperature.

[0017] The addition of urea can not only improve the thermoplastic processability of chitosan, but also improve the flexibility of thermoplastic chitosan materials. Urea molecules can combine with hydroxyl and amino groups in chitosan to form hydrogen bonds, thereby reducing the hydrogen bonding effect between chitosan itself and promoting the thermoplastic processability of chitosan. During the processing, small urea molecules penetrate into the chitosan molecular chain, increasing the mobility of the chitosan molecular chain and improving the flexibility of chitosan.

[0018] At the same time, the network structure formed by hydrogen bonds between urea and chitosan and the amino groups on the urea molecules play a synergistic role in the adsorption of metal ions, compensating for the problem of decreased adsorption performance caused by the reduction of chitosan content.

[0019] In the preparation method of the present invention, the solid content of chitosan can be maintained at more than 50-60% by controlling the process conditions, and the metal ion adsorption effect is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a graph showing the effect of thermoplastic chitosan with different urea contents on Cr(VI) removal. DETAILED DESCRIPTION

[0021] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0022] Example

[0023] Chitosan with a weight average molecular weight of about 50,000 and a deacetylation degree of 85% is uniformly mixed with an aqueous hydrochloric acid solution and urea (the mass ratio of chitosan to hydrochloric acid solution is 1:1.5, urea accounts for 0%, 5%, 10%, 15% and 20% of the total mass of chitosan and urea, respectively, and the mass fraction of hydrochloric acid in the hydrochloric acid solution is 5%, 6%, 7% and 8%, respectively), poured into an internal mixer at 80°C and a stirring speed of 30rpm and mixed for 15 minutes to obtain thermoplastic chitosan.

[0024] Table 1 Mechanical properties of urea hydrochloride plasticized thermoplastic chitosan

[0025]

[0026]

[0027] Mechanical properties test

[0028] The obtained thermoplastic chitosan was placed in a hot press and pressed at 90°C to obtain a uniform and transparent film of thermoplastic chitosan, which was then sliced ​​to obtain dumbbell-shaped sheets. The material was balanced in a constant humidity chamber at room temperature and 60% RH for two weeks before being subjected to a tensile test on a tensile machine (6P-Ts 2000s, Shenzhen Gaopin Testing Equipment Co., Ltd.). According to ASTM D 882-81, the tensile speed was set to 5 mm min -1 , the fixture is 40mm. After the material breaks, its fracture strength (σ b ,MPa) and fracture growth rate (ε b , %), each group of samples was measured 5 times to obtain the average value. The test results are shown in Table 1.

[0029] As can be seen from Table 1, using hydrochloric acid as a solvent, the tensile strength and elongation at break of the thermoplastic chitosan material change with the increase of urea content. When the hydrochloric acid content is 5%, with the increase of urea content, the tensile strength and elongation at break of the material first increase gradually and then decrease gradually, and the urea content reaches the maximum value after about 10%. With the increase of urea content, the other three thermoplastic chitosan materials with different hydrochloric acid contents have similar rules with 5% hydrochloric acid content. This result shows that urea has a plasticizing effect on chitosan materials. When the urea content exceeds 10%, the content of chitosan decreases a lot, so the overall mechanical properties of the material decrease. With the increase of hydrochloric acid content, the tensile strength and elongation at break of the thermoplastic chitosan material increase. At the same time, it can be seen from the results in the table that the elongation at break of the chitosan material modified with only 8% hydrochloric acid is similar to that of the chitosan material modified with 6% hydrochloric acid and 10% urea, indicating that urea can play a synergistic plasticizing role with hydrochloric acid.

[0030] Adsorption performance test

[0031] Using 8% hydrochloric acid solution as a plasticizer, a series of thermoplastic chitosans were prepared by changing the urea content (urea accounted for 0%, 5%, 10%, 15% and 20% of the total mass of chitosan and urea, respectively), named CC0, CC5, C10, CC15 and CC20 (the number represents the content of urea in the composite material). Then, taking chromium ions as the object, the effect of different urea contents on the adsorption performance of chromium ions was explored.

[0032] The specific experimental steps are as follows: accurately weigh 0.1g of thermoplastic chitosan material and add it to a conical flask containing 100mL of 100mg / L potassium dichromate solution. Set the shaker temperature to 25℃, put the conical flask into the shaker, and take samples at intervals within the range of 0 to 60min. Then test the absorbance and concentration of the solution at different times.

[0033] The urea content was gradually increased, and the effect of different urea contents on Cr(VI) removal was studied with the Cr(VI) adsorption amount as an indicator. The results are as follows: Figure 1 As shown in the figure, the adsorption rate of thermoplastic chitosan material remains unchanged as the urea content increases. This may be because the physical mixing between urea and chitosan increases a part of the amino group, but as the urea content increases, the chitosan content decreases, and the number of amino and hydroxyl groups as adsorption sites also decreases. The two offset each other, resulting in the unchanged overall adsorption efficiency of the material.

[0034] For matters not mentioned above, the prior art applies.

[0035] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A melt processing method for urea plasticized thermoplastic chitosan adsorption film, characterized in that: Chitosan, urea and solvent are uniformly mixed and poured into an internal mixer for mixing to obtain thermoplastic chitosan, and the thermoplastic chitosan is hot-pressed to obtain a thermoplastic chitosan film.

2. The melt processing method of a urea plasticized thermoplastic chitosan adsorption film according to claim 1, characterized in that: The solvent includes one or more of dilute hydrochloric acid, acetic acid, and lactic acid.

3. The melt processing method of a urea plasticized thermoplastic chitosan adsorption film according to claim 1, characterized in that: When the acid solution is dilute hydrochloric acid, the mass fraction of the dilute hydrochloric acid is 5% to 8%.

4. The melt processing method of a urea plasticized thermoplastic chitosan adsorption film as claimed in claim 3, characterized in that: The mass ratio of chitosan to dilute hydrochloric acid is 1:1.

5.

5. The melt processing method of a urea plasticized thermoplastic chitosan adsorption film according to claim 1, characterized in that: When the mass fraction of the dilute hydrochloric acid is 5%, urea accounts for 10% of the total mass of chitosan and urea; when the mass fraction of the dilute hydrochloric acid is 6%, urea accounts for 5% to 20% of the total mass of chitosan and urea; when the mass fraction of the dilute hydrochloric acid is 7%, urea accounts for 5% to 10% of the total mass of chitosan and urea; when the mass fraction of the dilute hydrochloric acid is 8%, urea accounts for 10% to 20% of the total mass of chitosan and urea.

6. A melt processing method for a urea plasticized thermoplastic chitosan adsorption film according to any one of claims 1 to 5, characterized in that: The banburying temperature is 60-90° C. and the banburying time is 5-15 minutes.

7. A melt processing method for a urea plasticized thermoplastic chitosan adsorption film according to any one of claims 1 to 5, characterized in that: The deacetylation degree of the chitosan is in the range of greater than 85%.

8. A melt processing method for a urea plasticized thermoplastic chitosan adsorption film according to any one of claims 1 to 5, characterized in that: The weight average molecular weight of the chitosan is 50,000 to 200,000.

9. A urea plasticized thermoplastic chitosan adsorption film prepared by the preparation method according to any one of claims 1 to 8.

10. The urea plasticized thermoplastic chitosan adsorption film according to claim 9, characterized in that: The solid content of chitosan is more than 50%, and it is used to adsorb heavy metal ions.

Citation Information

Patent Citations

  • Chitosan film and preparation method thereof

    CN102691229A

  • Fusion processing method for preparing thermoplastic chitosan

    CN106903814A

  • Method for preparing thermoplastic chitosan by lactic acid melting

    CN109575369A

  • Chitosan membrane material prepared from chitosan solution with pH value of 6-8 and preparation method of chitosan membrane material

    CN111748111A