A softener for ultra-soft and degradable spunbond nonwoven fabrics and its preparation method and application

By using melt mixing of PBS or PBSA with other materials, and applying it during the spinning process, the problems of low strength and poor spinning properties of non-woven fabric materials during the spinning process are solved, and softness and biodecomposition are achieved. Improvement of sex, suitable for a variety of sanitary products.

CN118773918BActive Publication Date: 2024-11-19SHANDONG DAWN POLYMER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254314.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

During the spinning process, existing non-woven fabric materials have problems such as low melt strength of degradable materials, poor spinning properties, easy to break wires during spinning, and the non-woven fabric feels hard and rough.

Method used

Polybutylene succinate (PBS) or polysuccinate-adipate-butylene glycol (PBSA) is used as the main materials, combining hydroxymethylcellulose, polyethylene glycol, aliphatic polyamide, Montan wax, ricinoleic acid, glyceryl monostearate is melted and mixed by a twin screw extruder to prepare a softener and add it to the modified material to improve the softness of the nonwoven fabric through specific ratios and process flow. and biodecomposition rate.

Benefits of technology

The softness and biodecomposition rate of non-woven fabrics have been significantly improved, so that their biodecomposition rate is greater than 95.3% in 180 days under composting conditions, and the fiber straight line is 18-19μm, which is suitable for infants and young children's diapers, feminine hygiene products and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773918B_ABST
    Figure CN118773918B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of degradable polymer materials, and more particularly to a softener for ultra-soft and degradable spunbond nonwoven fabrics, a preparation method and an application thereof. The softener is made of one of polybutylene succinate or polybutylene succinate-adipate, and is melt-mixed with hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid and glyceryl monostearate by a twin-screw extruder. Afterwards, the softener is used to prepare a modified material, and the modified material is used to prepare an ultra-soft and degradable spunbond nonwoven fabric, the nonwoven fabric having a softness of 16.5-19.7 mN, a fiber diameter of 18-19 μm, and a 180-day biodegradability rate greater than 95.3% under composting conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of degradable polymer materials, and in particular to a softener for ultra-soft and degradable spunbond nonwoven fabrics, and a preparation method and application thereof. Background Art

[0002] Nonwoven fabrics are the youngest and most promising emerging field in the textile industry. In the past half century, due to its characteristics of short process flow, high output, low cost, fast variety change, wide source of raw materials and excellent performance in many functions, it has gained great attention from the industry and favor from consumers. According to estimates, nonwoven fabrics are one of the upstream raw materials with the largest proportion in the cost of infant diapers, accounting for 26.9% of the production cost. With the popularization of scientific parenting concepts and the increase in consumption capacity, more and more parents use diapers, changing the habit of the older generation of hand-washing diapers. The market penetration rate of diapers is expected to increase from the current 60% to more than 80%, showing an overall steady growth trend.

[0003] The non-woven material used in diapers is polypropylene (PP). PP non-woven fabrics are hard to the touch, which results in the surface material of the prepared diapers being soft and the edges being hard, which in turn causes friction and scratches on the delicate skin on the inner thighs of infants and young children. In addition, PP non-woven fabrics cannot be degraded after use, and accumulate more and more in the environment, causing serious harm to the ecological environment. Fully biodegradable non-woven fabrics can be completely degraded into carbon dioxide and water after use and will not cause pollution to the environment.

[0004] Degradable materials have attracted widespread attention in recent years because they can be degraded into carbon dioxide and water after use and will not cause any pollution to the environment. However, among many biodegradable materials such as thermoplastic biodegradable plastics, which are copolymers of butylene adipate and butylene terephthalate (PBAT), polylactic acid (PLA), polycaprolactone (PCL), polyunsaturated phospholipid choline (PPC), polyhydroxyalkanoate (PHA), most materials have poor spinnability and the materials themselves cannot meet the spinning requirements. For example, the article "Research Progress of Preparation of PBS Degradable Composite Materials with Cellulose-based Fillers" in the journal "China Papermaking" was written by Wei Jiale and others. The article disclosed that cellulose has low cost and excellent mechanical properties, while polybutylene succinate (PBS) has good biocompatibility and degradability. Both are ideal polymer materials for preparing degradable composite materials. The article "Preparation and Properties of Fully Biodegradable High Impact PLA / PBAT Composite Materials" in the Journal of Liaoning Petrochemical University, written by Jiang Wenxin and others, disclosed that PLA has poor toughness, especially poor impact resistance, which limits its application range.

[0005] CN108823977A discloses a method for preparing an antibacterial PLA nonwoven fabric, comprising the following steps: pre-treating a PLA nonwoven fabric to obtain a first standby PLA nonwoven fabric; subjecting the first standby PLA nonwoven fabric to medium treatment to obtain a second standby PLA nonwoven fabric; preparing a cationic nano-silver solution; placing the second standby PLA nonwoven fabric into the cationic nano-silver solution for treatment to obtain a third standby PLA nonwoven fabric; and obtaining a PLA nano-silver nonwoven fabric based on the third standby PLA nonwoven fabric. However, this technical solution uses PLA materials with good spinning performance, and currently there are also problems such as brittle nonwoven fabric, poor toughness, low elongation, and poor fabric feel.

[0006] CN113106625A discloses a one-step method for preparing a degradable PBAT melt-blown nonwoven fabric, comprising the following steps: step 1: preparing a PBAT melt; step 2: preparing a modified PBAT melt; step 3: conveying the modified PBAT blended melt obtained in step 2 to a nonwoven fabric preparation device, wherein the melt in the nonwoven fabric preparation device is extruded from a spinneret hole of a die head and condensed on a roller-type receiver 4 cm away from the nozzle, wherein the roller speed of the receiver is 20 r / min, and the nonwoven fabric is self-bonded into a nonwoven fabric, and after cooling, the nonwoven fabric is removed from the roller with a blade and placed in a drying oven for drying and shaping, wherein the shaping temperature is 65° C. and the shaping time is 6 hours, thereby obtaining a PBAT melt-blown biodegradable nonwoven fabric. The present invention prepares degradable PBAT non-woven fabrics through a one-step method. Since the PBAT polymer melt does not need to go through water-cooled pelletizing, drying and cooling, heating and melting and mixing, etc., it avoids the decrease in PBAT resin molecular weight, viscosity reduction, and deterioration of melt quality caused by drying factors and high-temperature shearing, which can ensure the spinnability of the material and the quality of the PBAT non-woven fabric. This technical solution uses the melt-blowing method to prepare PBAT non-woven fabrics, but due to the slow cooling speed of PBAT, the spunbond method will produce sticky yarns during the yarn drawing process.

[0007] Based on the above-mentioned prior art, the non-woven fabrics in the prior art have technical problems that need to be solved urgently, such as low melt strength of degradable materials, poor spinnability, easy yarn breakage during the spinning process, and hard and rough touch of the non-woven fabrics. Summary of the invention

[0008] In order to solve the above technical problems, the present invention provides a super-soft and degradable softener for spunbonded non-woven fabrics. The softener is prepared by melt mixing one of polybutylene succinate (PBS) or polybutylene succinate-adipate (PBSA) with hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid and glyceryl monostearate through a twin-screw extruder. The melt index of the softener is 100-600g / 10min when the temperature and load are 190°C and 2.16kg respectively.

[0009] Furthermore, by weight, the components and contents of the softener are as follows:

[0010] Polybutylene succinate or polybutylene succinate-adipate: 60-80 parts by weight;

[0011] Hydroxymethyl cellulose: 3-5 parts by weight;

[0012] Polyethylene glycol: 5-8 parts by weight;

[0013] Aliphatic polyamide: 3-5 parts by weight;

[0014] Montan wax: 5-10 parts by weight;

[0015] Ricinoleic acid: 2-5 parts by weight;

[0016] Glyceryl monostearate: 3-5 parts by weight.

[0017] Furthermore, the melt index of the polybutylene succinate or polybutylene succinate-adipate is 26-39 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

[0018] The present invention also provides a method for preparing the above-mentioned ultra-soft and degradable spunbond nonwoven fabric softener, comprising the following steps:

[0019] Step 1, mixing hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate according to a certain proportion to obtain a softening agent premix;

[0020] Step 2: Add the prefabricated mixture of polybutylene succinate or polybutylene succinate-adipate and the softening aid prepared in step 1 into a twin-screw extruder for extrusion to obtain a softener.

[0021] Furthermore, the equipment used for mixing in step 1 is a high-speed mixer with a rotation speed of 300-800 rpm and a mixing time of 3-5 min.

[0022] Furthermore, the polybutylene succinate or polybutylene succinate-adipate-butylene glycol ester in step 2 enters the twin-screw extruder through a main feeding system connected to the first zone of the twin-screw extruder, and the softening aid premix enters the twin-screw extruder through a side feeding system connected to the fourth zone of the twin-screw extruder.

[0023] Furthermore, the twin-screw extruder used to prepare the softener includes thirteen temperature zones, and the temperatures of each zone are set to 110-120°C in zone one, 130-140°C in zone two, 150-160°C in zone three, 160-170°C in zone four, 160-170°C in zone five, 170-170°C in zone six, 170-180°C in zone seven, 170-180°C in zone eight, 170-180°C in zone nine, 170-180°C in zone ten, 170-180°C in zone eleven, 170-180°C in zone twelve, and 170-180°C in zone thirteen, the screw speed is 200-300r / min, the feeding rate is 30-50Hz, and the aspect ratio is 52:1.

[0024] Furthermore, the screw assembly in the twin-screw extruder includes at least one group of SME screw elements and at least one group of ZME screw elements.

[0025] Further, the screw assembly in the twin-screw extruder includes three groups of SME screw elements and three groups of ZME screw elements;

[0026] Among them, the first group of SME threaded elements corresponds to the second zone of the twin screw extruder, the second group of SME threaded elements corresponds to the sixth zone of the twin screw extruder, and the third group of SME threaded elements corresponds to the eleventh zone of the twin screw extruder; the first group of ZME threaded elements corresponds to the third zone of the twin screw extruder, the second group of ZME threaded elements corresponds to the sixth zone of the twin screw extruder, and the third group of ZME threaded elements corresponds to the tenth zone of the twin screw extruder.

[0027] Or the first group of SME threaded elements corresponds to zone one of the twin screw extruder, the second group of SME threaded elements corresponds to zone eight of the twin screw extruder, and the third group of SME threaded elements corresponds to zone twelve of the twin screw extruder; the first group of ZME threaded elements corresponds to zone two of the twin screw extruder, the second group of ZME threaded elements corresponds to zone seven of the twin screw extruder, and the third group of ZME threaded elements corresponds to zone ten of the twin screw extruder.

[0028] Furthermore, step 2 also includes granulation and drying after extrusion, wherein the equipment used for granulation is a granulator, and drying is drying to remove moisture.

[0029] The present invention also provides a modified material for super-soft and degradable spunbond non-woven fabrics. The modified material is prepared by melt-mixing one or two of polybutylene succinate-adipate (PBSA) or polybutylene succinate (PBS), a softener for the super-soft and degradable spunbond non-woven fabrics, a nucleating agent, a melt enhancer, and a thermal stabilizer. The melt index of the modified material is 21-42 g / 10 min when the temperature and load are 190° C. and 2.16 kg, respectively.

[0030] Furthermore, in parts by weight, the components and contents in the modified material are as follows:

[0031] Polybutylene succinate-adipate: 5-90 parts by weight;

[0032] Polybutylene succinate: 5-90 parts by weight;

[0033] Softener: 3-10 parts by weight;

[0034] Nucleating agent: 0.5-1.0 parts by weight;

[0035] Melt enhancer: 1.0-2.0 parts by weight;

[0036] Heat stabilizer: 0.5-1.0 parts by weight.

[0037] Furthermore, the melt index of the polybutylene succinate-adipate ester is 22-44 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

[0038] Furthermore, the melt index of the polybutylene succinate is 18-31 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

[0039] Furthermore, the nucleating agent is one of dibenzoyl hydrazide sebacic acid, attapulgite clay, and calcium phenylphosphonate.

[0040] Furthermore, the melt enhancer is one of 1,3-PBO dioxazoline compounds, diphenylmethane diisocyanate, and acrylic ester copolymers.

[0041] Furthermore, the heat stabilizer is a mixture of distearyl thiodipropionate and bis(3,5-di-tert-butyl-4-hydroxypropionyl)hydrazine in a mass ratio of 1:2.

[0042] The present invention also provides a method for preparing a modified material for ultra-soft and degradable spunbond nonwoven fabric, comprising the following steps:

[0043] Step 1, one or two of poly(butylene succinate-adipate) or poly(butylene succinate), the above-mentioned ultra-soft and degradable spunbond nonwoven fabric softener, nucleating agent, melt enhancer, and thermal stabilizer are mixed in proportion to obtain a modified material premix;

[0044] Step 2: Add the pre-made mixture of the modified material into a twin-screw extruder for extrusion to obtain the modified material.

[0045] Furthermore, the equipment used for mixing in step 1 is a high-speed mixer with a rotation speed of 500-800 rpm and a mixing time of 3-5 min.

[0046] Furthermore, the modified material premix in step 2 enters the twin-screw extruder through a main feeding system connected to a first zone of the twin-screw extruder;

[0047] Furthermore, the twin-screw extruder used to prepare the modified material includes eleven temperature zones, and the temperatures of each zone are set to 90-110°C in zone one, 100-130°C in zone two, 150-160°C in zone three, 150-160°C in zone four, 150-160°C in zone five, 170-180°C in zone six, 170-190°C in zone seven, 170-190°C in zone eight, 170-190°C in zone nine, 170-190°C in zone ten, and 170-190°C in zone eleven, the screw speed is 200-400r / min, the feeding rate is 10-30Hz, and the aspect ratio is 44:1.

[0048] Furthermore, step 2 also includes granulation and drying after extrusion, wherein the equipment used for granulation is a granulator, and drying is drying to remove moisture.

[0049] The present invention also provides a super soft and degradable spunbond nonwoven fabric, which is prepared from the modified material for the super soft and degradable spunbond nonwoven fabric. The nonwoven fabric has a softness of 16.5-19.7 mN, a fiber diameter of 18-19 μm, and a 180-day biodegradability rate greater than 95.3% under composting conditions.

[0050] The present invention also provides a method for preparing the above-mentioned super-soft and degradable spunbond non-woven fabric, comprising the following steps: adding the above-mentioned modified material for super-soft and degradable spunbond non-woven fabric into spunbond non-woven fabric production equipment, and obtaining the non-woven fabric by drawing and stretching.

[0051] Furthermore, the spunbond nonwoven fabric production equipment includes a single-screw extruder, and the modified material enters the single-screw extruder through a main feeding system connected to a first zone of the single-screw extruder.

[0052] Further, the single screw extruder comprises six temperature zones, and the temperature of each zone is set to 180-200°C for zone 1, 190-200°C for zone 2, 190-210°C for zone 3, 180-190°C for zone 4, 190-210°C for zone 5, and 180-190°C for zone 6;

[0053] At the same time, the die temperature is set to 190-210°C, the feed metering pump operates at a frequency of 15-30Hz, the non-woven fabric laying frequency is set to 40-60Hz, and the drafting frequency is 40-55Hz.

[0054] The present invention also provides a non-woven fabric product, which is prepared from the super-soft and degradable spunbonded non-woven fabric.

[0055] Furthermore, the non-woven fabric products include baby diapers, feminine hygiene products, face towels, facial masks, and wet wipes.

[0056] The beneficial effects of the present invention are:

[0057] 1. The softener prepared by the present invention is prepared by a specific raw material formula and ratio, in particular, a specific proportion of polybutylene succinate (PBS) or polybutylene succinate-adipate (PBSA) which is completely biodegradable, has excellent toughness, and has a melt index of 26-39 g / 10 min at a temperature and a load of 190° C. and 2.16 kg, respectively, is added thereto, and the components used to prepare the softener are fed in different feeding systems, melt-mixed and extruded by a specific twin-screw extruder to obtain a softener with a melt index of 100-600 g / 10 min at a temperature and a load of 190° C. and 2.16 kg, respectively; the softener is then added to the modified material, so that in the process of preparing the non-woven fabric, The first step is to form a stable raw material formula with one or both of the newly added polybutylene succinate-adipate (PBSA) or polybutylene succinate (PBS), thereby ensuring that the softener migrates outward in the fiber and migrates to the fiber surface during drawing and stretching, so that the softness of the non-woven fabric is significantly improved, and finally a non-woven fabric with a soft touch is obtained, that is, the softness of the non-woven fabric is 16.5-19.7 mN, the fiber diameter is 18-19 μm, and the biodegradability rate of the non-woven fabric under composting conditions is greater than 95.3% in 180 days. Under the same weaving conditions, the smaller the fiber diameter, the better the softness of the non-woven fabric. Therefore, the softer non-woven fabric prepared by the present invention can be widely used in the fields of baby diapers, female hygiene products, face towels, facial masks, wet wipes, etc.

[0058] 2. In the process of preparing a softener and using the softener to prepare a modified material, the present invention unexpectedly found that by using PBS or PBSA with a high melt index (the melt index is 26-39 g / 10 min when the temperature and load are 190°C and 2.16 kg respectively), a high melt index softener can be obtained, and the non-woven fabric has good spinning stability. Finally, the existing process for preparing the non-woven fabric is simplified, and a preparation method with a simple process route, high spinning stability, and easy industrial production is obtained;

[0059] 3. In the process of preparing the softener, the raw materials are specifically mixed and fed in different zones, that is, the polybutylene succinate or polybutylene succinate-adipate-butylene glycol ester enters the twin-screw extruder through the main feeding system connected to the first zone of the twin-screw extruder, and the prefabricated mixture of the softening aid enters the twin-screw extruder through the side feeding system connected to the fourth zone of the twin-screw extruder. It is unexpectedly found that the dispersion degree is better than that of feeding all the raw materials together after mixing, which further improves the preparation of subsequent modified materials and non-woven fabrics. At the same time, the screw combination in the twin-screw extruder includes at least one group of SME thread elements and at least one group of ZME thread elements to achieve weak shearing and strong dispersion of each component in the softener, thereby obtaining a softener with high dispersion and can be used in the preparation process of ultra-soft and degradable spunbond non-woven fabrics;

[0060] 4. In the process of preparing the modified material of the present invention, a softener with a specific melt index is first prepared, and then 1,3-PBO dioxazoline compounds, diphenylmethane diisocyanate, and one of acrylic ester copolymers are specifically added as a melt enhancer to further improve the melt strength of the modified material. In the process of preparing the non-woven fabric, the yarn breakage during the spinning process can be avoided. Compared with the non-woven fabric in which the raw materials are mixed and spun together in the prior art, under the same spinning conditions, the non-woven fabric prepared by the present invention has a finer fiber diameter and better softness. In addition, the softener and the modified material obtained before preparing the non-woven fabric can be stably stored, thereby ensuring stable production again, and is more suitable for the preparation of non-woven fabrics on production lines with high output. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 The nonwoven fabric sample prepared in Example 5 of the present invention;

[0062] Figure 2 This is a scanning electron microscope image of the nonwoven fabric prepared in Example 5 of the present invention;

[0063] Figure 3 This is a scanning electron microscope image of the nonwoven fabric prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0064] Examples 1-2 are softeners for ultra-soft and degradable spunbond nonwoven fabrics and a preparation method thereof, Examples 3-4 are modified materials for ultra-soft and degradable spunbond nonwoven fabrics prepared from the softeners prepared from Examples 1-2 and a preparation method thereof, and Examples 5-6 are ultra-soft and degradable spunbond nonwoven fabrics prepared from the modified materials prepared from Examples 3-4 and a preparation method thereof.

[0065] The melt index determination standard involved in the present invention is ASTM D1238; the softness determination standard is GB / T2986-2016; and the fiber diameter is determined by scanning electron microscopy.

[0066] Example 1

[0067] The present embodiment provides a softener for ultra-soft and biodegradable spunbond nonwoven fabrics. The softener is prepared by melt mixing polybutylene succinate-adipate (PBSA), hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate through a twin-screw extruder. The melt index of the softener is 102 g / 10 min when the temperature and load are 190° C. and 2.16 kg, respectively.

[0068] By weight, the components and contents of the softener are as follows:

[0069] Polybutylene succinate-adipate: 60 parts by weight;

[0070] Hydroxymethyl cellulose: 5 parts by weight;

[0071] Polyethylene glycol: 8 parts by weight;

[0072] Aliphatic polyamide: 3 parts by weight;

[0073] Montan wax: 5 parts by weight;

[0074] Ricinoleic acid: 2 parts by weight;

[0075] Glyceryl monostearate: 3 parts by weight.

[0076] In this embodiment, the melt index of the polybutylene succinate-adipate ester at a temperature and a load of 190° C. and 2.16 kg is 26 g / 10 min.

[0077] This embodiment also provides a method for preparing the above-mentioned ultra-soft and degradable spunbond nonwoven fabric softener, comprising the following steps:

[0078] Step 1, mixing hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate according to a certain proportion to obtain a softening agent premix;

[0079] The mixing equipment used is a high-speed mixer with a rotation speed of 300 rpm and a mixing time of 5 min;

[0080] Step 2, adding the prefabricated mixture of polybutylene succinate-adipate and the softening aid prepared in step 1 into a twin-screw extruder for extrusion to obtain an extrudate, and granulating and drying to obtain a softener;

[0081] The polybutylene succinate-adipate ester enters the twin-screw extruder through a main feeding system connected to the first zone of the twin-screw extruder, and the preformed softening agent mixture enters the twin-screw extruder through a side feeding system connected to the fourth zone of the twin-screw extruder;

[0082] Wherein, the twin-screw extruder used to prepare the softener includes thirteen temperature zones, and the temperatures of the zones are set to 110°C for zone 1, 130°C for zone 2, 150°C for zone 3, 170°C for zone 4, 160°C for zone 5, 170°C for zone 6, 180°C for zone 7, 170°C for zone 8, 170°C for zone 9, 170°C for zone 10, 180°C for zone 11, 170°C for zone 12, and 170°C for zone 13, respectively. The screw speed is 200r / min, the feeding speed is 30Hz, and the aspect ratio is 52:1;

[0083] In this embodiment, special elements, namely three groups of SME screw elements and three groups of ZME screw elements, are introduced into the screw assembly in the twin-screw extruder;

[0084] Among them, the first group of SME threaded elements corresponds to zone one of the twin screw extruder, the second group of SME threaded elements corresponds to zone eight of the twin screw extruder, and the third group of SME threaded elements corresponds to zone twelve of the twin screw extruder; the first group of ZME threaded elements corresponds to zone two of the twin screw extruder, the second group of ZME threaded elements corresponds to zone seven of the twin screw extruder, and the third group of ZME threaded elements corresponds to zone ten of the twin screw extruder.

[0085] Example 2

[0086] This embodiment provides a super-soft and degradable softener for spunbond nonwoven fabrics, wherein the softener is prepared by melt mixing polybutylene succinate (PBS), hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate through a twin-screw extruder, and the melt index of the softener is 579 g / 10 min when the temperature and load are 190° C. and 2.16 kg, respectively;

[0087] By weight, the components and contents of the softener are as follows:

[0088] Polybutylene succinate: 80 parts by weight;

[0089] Hydroxymethyl cellulose: 3 parts by weight;

[0090] Polyethylene glycol: 5 parts by weight;

[0091] Aliphatic polyamide: 5 parts by weight;

[0092] Montan wax: 10 parts by weight;

[0093] Ricinoleic acid: 2 parts by weight;

[0094] Glyceryl monostearate: 5 parts by weight.

[0095] In this embodiment, the melt index of the polybutylene succinate at a temperature and a load of 190° C. and 2.16 kg is 39 g / 10 min.

[0096] This embodiment also provides a method for preparing the above-mentioned ultra-soft and degradable spunbond nonwoven fabric softener, comprising the following steps:

[0097] Step 1, mixing hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate according to a certain proportion to obtain a softening agent premix;

[0098] The mixing equipment used is a high-speed mixer with a rotation speed of 800 rpm and a mixing time of 3 min;

[0099] Step 2, adding the prefabricated mixture of polybutylene succinate and the softening aid prepared in step 1 into a twin-screw extruder for extrusion to obtain an extrudate, and granulating and drying to obtain a softener;

[0100] The polybutylene succinate enters the twin-screw extruder through a main feeding system connected to the first zone of the twin-screw extruder, and the prefabricated mixture of the softening aid enters the twin-screw extruder through a side feeding system connected to the fourth zone of the twin-screw extruder;

[0101] Wherein, the twin-screw extruder used to prepare the softener includes thirteen temperature zones, and the temperatures of the zones are set to 120°C for zone 1, 140°C for zone 2, 160°C for zone 3, 160°C for zone 4, 170°C for zone 5, 180°C for zone 6, 170°C for zone 7, 180°C for zone 8, 180°C for zone 9, 180°C for zone 10, 170°C for zone 11, 180°C for zone 12, and 180°C for zone 13, respectively. The screw speed is 300r / min, the feeding speed is 50Hz, and the aspect ratio is 52:1;

[0102] In this embodiment, special elements are introduced into the screw assembly in the twin-screw extruder, namely, three groups of SME screw elements and three groups of ZME screw elements;

[0103] Among them, the first group of SME threaded elements corresponds to the second zone of the twin screw extruder, the second group of SME threaded elements corresponds to the sixth zone of the twin screw extruder, and the third group of SME threaded elements corresponds to the eleventh zone of the twin screw extruder; the first group of ZME threaded elements corresponds to the third zone of the twin screw extruder, the second group of ZME threaded elements corresponds to the sixth zone of the twin screw extruder, and the third group of ZME threaded elements corresponds to the tenth zone of the twin screw extruder.

[0104] Example 3

[0105] This embodiment uses the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 1 to prepare an ultra-soft and degradable spunbond nonwoven fabric modified material. The modified material is made by melt-mixing polybutylene succinate-adipate (PBSA), polybutylene succinate (PBS), the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 1, a nucleating agent, a melt enhancer, and a thermal stabilizer. The melt index of the modified material is 42 g / 10 min when the temperature and load are 190° C. and 2.16 kg, respectively.

[0106] By weight, the components and contents in the modified material are as follows:

[0107] Polybutylene succinate-adipate: 90 parts by weight;

[0108] Polybutylene succinate: 5 parts by weight;

[0109] Softener prepared in Example 1: 3 parts by weight;

[0110] Nucleating agent sebacic acid dibenzoyl hydrazide: 0.5 parts by weight;

[0111] Melt enhancer diphenylmethane diisocyanate: 1.0 parts by weight;

[0112] Heat stabilizer: 0.5 parts by weight, which is a mixture of distearyl thiodipropionate and bis(3,5-di-tert-butyl-4-hydroxypropionyl)hydrazine in a mass ratio of 1:2.

[0113] In this embodiment, the melt index of the polybutylene succinate-adipate ester is 22 g / 10 min at a temperature and a load of 190° C. and 2.16 kg;

[0114] The polybutylene succinate has a melt index of 18 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

[0115] This embodiment also provides a method for preparing the modified material for the ultra-soft and degradable spunbond nonwoven fabric, comprising the following steps:

[0116] Step 1, polybutylene succinate-adipate, polybutylene succinate, the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 1, a nucleating agent, a melt enhancer, and a heat stabilizer are mixed according to a proportion to obtain a modified material premix;

[0117] The mixing equipment used is a high-speed mixer with a rotation speed of 500 rpm and a mixing time of 3 min;

[0118] Step 2, adding the pre-made mixture of the modified material into a twin-screw extruder for extrusion to obtain an extruded material, and granulating and drying to obtain a modified material;

[0119] The modified material premix enters the twin-screw extruder through a main feeding system connected to a first zone of the twin-screw extruder;

[0120] Among them, the twin-screw extruder used to prepare the modified material includes eleven temperature zones, and the temperatures of each zone are set to 110°C in zone 1, 130°C in zone 2, 150°C in zone 3, 160°C in zone 4, 160°C in zone 5, 170°C in zone 6, 170°C in zone 7, 170°C in zone 8, 170°C in zone 9, 170°C in zone 10, and 190°C in zone 11. The screw speed is 200r / min, the feeding speed is 30Hz, and the aspect ratio is 44:1.

[0121] Example 4

[0122] This embodiment uses the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 2 to prepare an ultra-soft and degradable spunbond nonwoven fabric modified material. The modified material is made by melt-mixing polybutylene succinate-adipate (PBSA), polybutylene succinate (PBS), the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 2, a nucleating agent, a melt enhancer, and a thermal stabilizer. The melt index of the modified material is 21 g / 10 min at a temperature and a load of 190°C and 2.16 kg.

[0123] By weight, the components and contents in the modified material are as follows:

[0124] Polybutylene succinate-adipate: 5 parts by weight;

[0125] Polybutylene succinate: 90 parts by weight;

[0126] Softener prepared in Example 2: 10 parts by weight;

[0127] Nucleating agent calcium phenylphosphonate: 1.0 parts by weight;

[0128] Melt enhancer 1,3-PBO dioxazoline: 2.0 parts by weight;

[0129] Heat stabilizer: 1.0 part by weight, which is a mixture of distearyl thiodipropionate and bis(3,5-di-tert-butyl-4-hydroxypropionyl)hydrazine in a mass ratio of 1:2.

[0130] In this embodiment, the melt index of the polybutylene succinate-adipate ester is 44 g / 10 min at a temperature and a load of 190° C. and 2.16 kg;

[0131] The polybutylene succinate had a melt index of 31 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

[0132] This embodiment also provides a method for preparing the modified material for the ultra-soft and degradable spunbond nonwoven fabric, comprising the following steps:

[0133] Step 1, polybutylene succinate-adipate, polybutylene succinate, the ultra-soft and degradable spunbond nonwoven fabric softener prepared in Example 1, a nucleating agent, a melt enhancer, and a heat stabilizer are mixed according to a proportion to obtain a modified material premix;

[0134] The mixing equipment used is a high-speed mixer with a rotation speed of 800 rpm and a mixing time of 5 min;

[0135] Step 2, adding the pre-made mixture of the modified material into a twin-screw extruder for extrusion to obtain an extruded material, and granulating and drying to obtain a modified material;

[0136] The modified material premix enters the twin-screw extruder through a main feeding system connected to a first zone of the twin-screw extruder;

[0137] Among them, the twin-screw extruder used to prepare the modified material includes eleven temperature zones, and the temperatures of each zone are set to 90°C in zone one, 100°C in zone two, 160°C in zone three, 150°C in zone four, 150°C in zone five, 180°C in zone six, 190°C in zone seven, 190°C in zone eight, 190°C in zone nine, 190°C in zone ten, and 170°C in zone eleven. The screw speed is 400r / min, the feeding speed is 10Hz, and the aspect ratio is 44:1.

[0138] Example 5

[0139] This embodiment provides a super soft and degradable spunbond nonwoven fabric, such as Figure 1 The nonwoven fabric is prepared from the modified material of the ultra-soft and degradable spunbond nonwoven fabric prepared in Example 3. The nonwoven fabric has a softness of 16.5 mN and a biodegradability rate of 95.3% in 180 days under composting conditions. Figure 2 The figure shows a scanning electron microscope image of the nonwoven fabric, and the average fiber diameter is 18.5 μm. This embodiment also provides a method for preparing the above-mentioned ultra-soft and degradable spunbond nonwoven fabric, comprising the following steps: adding the modified material for ultra-soft and degradable spunbond nonwoven fabric prepared in Example 3 to a spunbond nonwoven fabric production device, and obtaining the nonwoven fabric by drawing and stretching.

[0140] Wherein, the spunbond nonwoven fabric production equipment comprises a single screw extruder, and the modified material enters the single screw extruder through a main feeding system connected to a first zone of the single screw extruder;

[0141] The single screw extruder comprises six temperature zones, and the temperatures of the zones are respectively set at 180°C for zone 1, 190°C for zone 2, 190°C for zone 3, 190°C for zone 4, 190°C for zone 5, and 190°C for zone 6;

[0142] At the same time, the die temperature was set to 190°C, the feed metering pump operated at 15 Hz, the nonwoven fabric laying frequency was set to 40 Hz, and the drafting air frequency was 40 Hz.

[0143] Example 6

[0144] The present embodiment provides an ultra-soft and degradable spunbond nonwoven fabric, which is prepared from the modified material for the ultra-soft and degradable spunbond nonwoven fabric prepared in Example 4. The nonwoven fabric has a softness of 19.7 mN, a biodegradability rate of 95.6% in 180 days under composting conditions, and an average fiber diameter of 18.8 μm.

[0145] This embodiment also provides a method for preparing the above-mentioned ultra-soft and degradable spunbond non-woven fabric, comprising the following steps: adding the modified material for the ultra-soft and degradable spunbond non-woven fabric prepared in Example 4 to a spunbond non-woven fabric production device, and obtaining the non-woven fabric by drawing and stretching.

[0146] Wherein, the spunbond nonwoven fabric production equipment comprises a single screw extruder, and the modified material enters the single screw extruder through a main feeding system connected to a first zone of the single screw extruder;

[0147] The single screw extruder includes six temperature zones, and the temperatures of the zones are set to 200°C for zone 1, 200°C for zone 2, 210°C for zone 3, 180°C for zone 4, 210°C for zone 5, and 180°C for zone 6;

[0148] At the same time, the die temperature was set to 210°C, the feed metering pump operated at 30 Hz, the nonwoven fabric laying frequency was set to 60 Hz, and the drafting air frequency was 55 Hz.

[0149] Comparative Example 1

[0150] This comparative example is based on the softener preparation formula of Example 2, but without performing specific twin-screw feeding and extrusion granulation on the formula, and directly mixing the raw materials with the raw materials for preparing the modified material to prepare the modified material in this comparative example.

[0151] That is, this comparative example directly provides a modified material relative to Example 4, and the modified material is made by melt-mixing polybutylene succinate-adipate (PBSA), polybutylene succinate (PBS), the raw materials and proportions involved in the softener for ultra-soft and degradable spunbond non-woven fabric prepared in Example 2, a nucleating agent, a melt enhancer, and a thermal stabilizer. The melt index of the modified material is 15 g / 10 min when the temperature and load are 190°C and 2.16 kg respectively.

[0152] By weight, the components and contents in the modified material are as follows:

[0153] Polybutylene succinate-adipate: 5 parts by weight;

[0154] Polybutylene succinate: 90 parts by weight;

[0155] Softener: 3 parts by weight;

[0156] Nucleating agent sebacic acid dibenzoyl hydrazide: 0.5 parts by weight;

[0157] Melt enhancer diphenylmethane diisocyanate: 1.0 parts by weight;

[0158] Heat stabilizer: 0.5 parts by weight, which is a mixture of distearyl thiodipropionate and bis(3,5-di-tert-butyl-4-hydroxypropionyl)hydrazine in a mass ratio of 1:2.

[0159] In this comparative example, the melt index of the polybutylene succinate-adipate ester at a temperature and load of 190° C. and 2.16 kg is 26 g / 10 min;

[0160] The polybutylene succinate had a melt index of 26 g / 10 min at a temperature and a load of 190° C. and 2.16 kg.

[0161] Among them, the components and contents of the softener in this comparative example are:

[0162] Polybutylene succinate: 74 parts by weight;

[0163] Hydroxymethyl cellulose: 5 parts by weight;

[0164] Polyethylene glycol: 8 parts by weight;

[0165] Aliphatic polyamide: 3 parts by weight;

[0166] Montan wax: 5 parts by weight;

[0167] Ricinoleic acid: 2 parts by weight;

[0168] Glyceryl monostearate: 3 parts by weight.

[0169] In the formulation of the softener of this comparative example, the melt index of the polybutylene succinate is 26 g / 10 min at a temperature and a load of 190° C. and 2.16 kg, respectively.

[0170] This comparative example also provides a method for preparing the above-mentioned modified material, comprising the following steps:

[0171] Step 1, polybutylene succinate-adipate, polybutylene succinate, the raw materials involved in the ultra-soft and degradable spunbond nonwoven softener prepared in Example 2, a nucleating agent, a melt enhancer, and a heat stabilizer are mixed according to a proportion to obtain a modified material premix;

[0172] The mixing equipment used is a high-speed mixer with a rotation speed of 500 rpm and a mixing time of 3 min;

[0173] Step 2, adding the pre-made mixture of the modified material into a twin-screw extruder for extrusion to obtain an extruded material, and granulating and drying to obtain a modified material;

[0174] The modified material premix enters the twin-screw extruder through a main feeding system connected to a first zone of the twin-screw extruder;

[0175] Among them, the twin-screw extruder used to prepare the modified material includes eleven temperature zones, and the temperatures of each zone are set to 110°C in zone 1, 130°C in zone 2, 150°C in zone 3, 160°C in zone 4, 160°C in zone 5, 170°C in zone 6, 170°C in zone 7, 170°C in zone 8, 170°C in zone 9, 170°C in zone 10, and 170°C in zone 11, the screw speed is 200r / min, the feeding speed is 30Hz, and the aspect ratio is 44:1.

[0176] The performance of the modified material prepared in this comparative example was compared with that of Examples 3-4, and the comparison results are shown in Table 1:

[0177] Table 1 Comparison of melt index of modified materials prepared in Examples 3-4 and Comparative Example 1

[0178]

[0179] Comparative Example 2

[0180] This comparative example provides a non-woven fabric, which is prepared from the modified material prepared in comparative example 1. The non-woven fabric has a softness of 12.4 mN and a biodegradability of 94.5% in 180 days under composting conditions. Figure 3 The figure shows a scanning electron microscope image of the nonwoven fabric, and the average fiber diameter is 25.7 μm.

[0181] This comparative example also provides a method for preparing the above non-woven fabric, comprising the following steps: adding the modified material prepared in comparative example 1 into a spunbond non-woven fabric production device, and obtaining the non-woven fabric by drawing and stretching.

[0182] Wherein, the spunbond nonwoven fabric production equipment comprises a single screw extruder, and the modified material enters the single screw extruder through a main feeding system connected to a first zone of the single screw extruder;

[0183] The single screw extruder comprises six temperature zones, and the temperatures of the zones are respectively set at 180°C for zone 1, 190°C for zone 2, 190°C for zone 3, 190°C for zone 4, 190°C for zone 5, and 190°C for zone 6;

[0184] At the same time, the die temperature was set to 190°C, the feed metering pump operated at 15 Hz, the nonwoven fabric laying frequency was set to 40 Hz, and the drafting air frequency was 40 Hz.

[0185] The performance of the nonwoven fabric prepared in this comparative example was compared with that of Examples 5-6. The comparison results are shown in Table 2:

[0186] Table 2 Comparison of the properties of the nonwoven fabrics prepared in Examples 5-6 and Comparative Example 2

[0187]

[0188] Through the intuitive comparison of the embodiments and comparative examples and Table 1 and Table 2, it can be seen that the softener prepared by the present invention through a specific raw material formula and ratio, especially adding a specific proportion of polybutylene succinate (PBS) or polybutylene succinate-adipate (PBSA) which is completely biodegradable, has excellent toughness, and has a melt index of 26-39 g / 10 min at a temperature and a load of 190° C. and 2.16 kg, respectively, and the components used to prepare the softener are divided into different feeding systems for feeding, melt mixing and extrusion through a specific twin-screw extruder, to obtain a softener with a melt index of 100-600 g / 10 min at a temperature and a load of 190° C. and 2.16 kg, respectively; and then adding the softener to the modified material to make it at In the process of preparing the non-woven fabric, a stable raw material formula is formed again with one or both of the newly added polybutylene succinate-adipate (PBSA) or polybutylene succinate (PBS), thereby ensuring that the softener migrates outward in the fiber and migrates to the fiber surface during drawing and stretching, so that the softness of the non-woven fabric is significantly improved, and finally a non-woven fabric with a soft touch is obtained, that is, the softness of the non-woven fabric is 16.5-19.7mN, the fiber diameter is 18-19μm, and the biodegradability rate of the non-woven fabric in 180 days under composting conditions is greater than 95.3%. Under the same weaving conditions, the smaller the fiber diameter, the better the softness of the non-woven fabric. Therefore, the softer non-woven fabric prepared by the present invention can be widely used in the fields of baby diapers, feminine hygiene products, face towels, facial masks, wet wipes, etc.

[0189] It should be understood that the present invention is not limited to what has been described above and shown in the accompanying drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.

Claims

1. A modified material for ultra-soft and degradable spunbond nonwoven fabric, characterized in that: The modified material is prepared by melt mixing one or two of poly(butylene succinate-adipate-butylene succinate) or poly(butylene succinate), a softener for ultra-soft and degradable spunbond nonwoven fabric, a nucleating agent, a melt enhancer, and a heat stabilizer. The melt index of the modified material is 21-42 g / 10 min at a temperature of 190° C. and a load of 2.16 kg, respectively. By weight, the components and contents in the modified material are as follows: Polybutylene succinate-adipate: 5-90 parts by weight; Polybutylene succinate: 5-90 parts by weight; Softener: 3-10 parts by weight; Nucleating agent: 0.5-1.0 parts by weight; Melt enhancer: 1.0-2.0 parts by weight; Heat stabilizer: 0.5-1.0 parts by weight; The softener is prepared by melt mixing one of polybutylene succinate or polybutylene succinate-adipate, hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate through a twin-screw extruder, and the melt index of the softener is 100-600g / 10min when the temperature and load are 190°C and 2.16kg respectively; By weight, the components and contents of the softener are as follows: Polybutylene succinate or polybutylene succinate-adipate: 60-80 parts by weight; Hydroxymethyl cellulose: 3-5 parts by weight; Polyethylene glycol: 5-10 parts by weight; Aliphatic polyamide: 3-5 parts by weight; Montan wax: 5-10 parts by weight; Ricinoleic acid: 2-5 parts by weight; Glyceryl monostearate: 3-5 parts by weight; Wherein, the melt index of the polybutylene succinate or polybutylene succinate-adipate is 26-39 g / 10 min at a temperature of 190° C. and a load of 2.16 kg; The preparation method of the softener comprises the following steps: Step 1, mixing hydroxymethyl cellulose, polyethylene glycol, aliphatic polyamide, montan wax, ricinoleic acid, and glyceryl monostearate according to a certain proportion to obtain a softening agent premix; Step 2, adding the prefabricated mixture of polybutylene succinate or polybutylene succinate-adipate and the softening aid prepared in step 1 into a twin-screw extruder for extrusion to obtain a softener; Wherein, the polybutylene succinate or polybutylene succinate-adipate-butylene glycol ester in step 2 enters the twin-screw extruder through the main feeding system connected to the first zone of the twin-screw extruder, and the softening aid premix enters the twin-screw extruder through the side feeding system connected to the fourth zone of the twin-screw extruder.

2. The modified material for ultra-soft and degradable spunbond nonwoven fabric according to claim 1, characterized in that: The twin-screw extruder for preparing the softener comprises thirteen temperature zones, and the temperatures of the zones are respectively set to 110-120°C for zone one, 130-140°C for zone two, 150-160°C for zone three, 160-170°C for zone four, 160-170°C for zone five, 170-180°C for zone six, 170-180°C for zone seven, 170-180°C for zone eight, 170-180°C for zone nine, 170-180°C for zone ten, 170-180°C for zone eleven, 170-180°C for zone twelve, and 170-180°C for zone thirteen, the screw speed is 200-300r / min, the feeding speed is 30-50Hz, and the aspect ratio is 52:

1.

3. The modified material for ultra-soft and degradable spunbond nonwoven fabric according to claim 1, characterized in that: The melt index of the polybutylene succinate-adipate ester is 22-44 g / 10 min at a temperature of 190° C. and a load of 2.16 kg; The polybutylene succinate has a melt index of 18-31 g / 10 min at a temperature of 190° C. and a load of 2.16 kg.

4. The modified material for ultra-soft and degradable spunbond nonwoven fabric according to claim 1, characterized in that: The nucleating agent is one of dibenzoyl hydrazide sebacic acid, attapulgite clay, and calcium phenylphosphonate; The melt enhancer is one of 1,3-PBO dioxazoline compounds, diphenylmethane diisocyanate, and acrylic copolymers; The heat stabilizer is a mixture of distearyl thiodipropionate and bis(3,5-di-tert-butyl-4-hydroxypropionyl)hydrazine in a mass ratio of 1:

2.

5. A method for preparing the modified material for ultra-soft and degradable spunbond nonwoven fabric according to any one of claims 1 to 4, characterized in that: The steps include: Step 1, mixing one or two of poly(butylene succinate-adipate) or poly(butylene succinate), the softener for the ultra-soft and degradable spunbond nonwoven fabric according to claim 1, a nucleating agent, a melt enhancer, and a heat stabilizer according to a certain proportion to obtain a prefabricated mixture of a modified material; Step 2, adding the pre-made mixture of the modified material into a twin-screw extruder for extrusion to obtain the modified material; Wherein, the modified material premix in step 2 enters the twin-screw extruder through a main feeding system connected to a first zone of the twin-screw extruder.

6. A super soft and degradable spunbond nonwoven fabric, characterized in that: The non-woven fabric is prepared from the modified material for the ultra-soft and degradable spunbond non-woven fabric according to any one of claims 1 to 4, the non-woven fabric has a softness of 16.5-19.7 mN, a fiber diameter of 18-19 μm, and a 180-day biodegradability rate under composting conditions of greater than 95.3%.

7. A method for preparing the ultra-soft and degradable spunbond nonwoven fabric according to claim 6, characterized in that: The method comprises the following steps: adding the modified material for ultra-soft and degradable spunbond nonwoven fabrics according to any one of claims 1 to 4 into a spunbond nonwoven fabric production device, and obtaining the nonwoven fabrics by drawing and stretching.

8. A nonwoven fabric product, characterized in that: The non-woven fabric product is made from the ultra-soft and degradable spunbond non-woven fabric according to claim 6.