Solid superacid isomerization catalyst as well as preparation method and application thereof
By using a combined preparation method of monoclinic and tetragonal zirconia precursors and pseudo-boehmite and other materials, the problem of insufficient activity of solid superacid catalysts was solved, the process was simplified and industrialized, and the catalyst performance was improved. Performance and stability.
Patent Information
- Application Number
- CN202410858191.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
Existing solid superacid catalysts have insufficient activity and complex preparation methods, which increase production costs and require high equipment, making it difficult to achieve industrial production.
The zirconia precursor mixed with monoclinic and tetragonal phases is soaked and roasted with pseudo-boehmite and sulfuric acid solution, and combined with sesbania powder, silica sol and precious metal active components, the solid superacid isomer is prepared by an equal volume impregnation method. Chemical catalyst, simple process and low equipment requirements.
It improves the activity, selectivity and stability of the catalyst, reduces process energy consumption, and reduces by-product waste. It is suitable for industrial production and has excellent catalytic performance and applicability.
Smart Images

Figure CN118847162A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a solid superacid isomerization catalyst and a preparation method and application thereof. Background Art
[0002] With the rapid development of modern industry, people's awareness of environmental protection has gradually increased, and the development of clean gasoline has received more and more attention. Obtaining clean gasoline with low sulfur, low aromatics, low olefins and high octane number has become the future development direction. Improving the quality and anti-knock properties of gasoline, increasing the octane number of gasoline, and reducing the impact of gasoline use on the environment rely on high-performance isomerization catalysts. Since 1979, Japanese Hino et al. reported SO4 2- / M x O y After the solid superacid catalyst was successfully used in the isomerization reaction of n-butane, people gradually focused on this catalyst with high catalytic activity and few by-products.
[0003] A large amount of C5 / C6 light hydrocarbon components will be produced during the processing of crude oil. Isomerization of light alkanes is the most important method to increase the octane number. Isomerization catalysts are the core of isomerization technology. Common catalysts can be divided into medium-temperature molecular sieve catalysts, low-temperature Pt-Cl / AlCl3 catalysts and solid superacid catalysts. Medium-temperature molecular sieve catalysts mainly use molecular sieves as carriers and load precious metals as active components. They have good anti-toxicity and regeneration, but their reaction temperature is high, resulting in low product octane number. Low-temperature Pt-Cl / AlCl3 catalysts have high activity at low temperatures and high product octane number, but chlorine needs to be continuously supplemented during the operation of the catalyst, which is easy to corrode the equipment. At the same time, the requirements for the reaction raw materials are high, and a small amount of water and sulfur will cause the catalyst to deactivate. Solid superacid catalysts are highly acidic, have high activity at low temperature and low pressure, are regenerable and have low equipment requirements, and have great development prospects.
[0004] The work of many researchers has promoted the development of solid superacid isomerization catalysts. For example, patent CN1299299A discloses a single tetragonal zirconium oxide superacid solid catalyst, the grain size of ZrO2 is about 3.0nm, and the specific surface area is 298m 2 / g, it has the characteristics of low reaction temperature, high equilibrium conversion rate, good selectivity, etc., but its activity is relatively insufficient. The relevant literature uses a hydrothermal method to modify zirconium hydroxide to prepare a solid superacid catalyst, compares the effect of hydrothermal temperature on the preparation of hydrated zirconium oxide, and finds that the crystalline hydrated zirconium oxide obtained by the hydrothermal method has a high catalytic activity when used to prepare a solid superacid catalyst. In the existing methods for preparing solid superacid catalysts, zirconium hydroxide or zirconium oxide prepared by reacting zirconium salts with precipitants such as ammonia water is generally used as a raw material, and a large amount of water is required to wash the acid ions, otherwise the activity is insufficient, which increases the production cost. Therefore, it is necessary to develop a method for preparing a solid superacid isomerization catalyst, which has a simple process, is easy to realize industrial production, and the catalyst has good activity and selectivity. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a solid superacid isomerization catalyst and a preparation method and application thereof.
[0006] In a first aspect, the present invention provides a method for preparing a solid superacid isomerization catalyst, the preparation method comprising the following steps:
[0007] A monoclinic and tetragonal mixed zirconium oxide precursor is obtained;
[0008] The zirconium oxide precursor and pseudo-boehmite are mixed, and then a sulfuric acid solution is added for soaking, filtering, drying, grinding and first calcining to obtain a carrier precursor;
[0009] The carrier precursor, sesbania powder, silica sol, acid solution and water are kneaded and then extruded, and then placed at room temperature, dried and second calcined to obtain a catalyst carrier;
[0010] The noble metal active component is impregnated on the catalyst carrier by adopting an equal volume impregnation method, and then aging and a third calcination are performed to obtain the solid superacid isomerization catalyst.
[0011] Furthermore, the step of obtaining a monoclinic and tetragonal mixed zirconium oxide precursor comprises the following process:
[0012] Dissolve zirconium oxychloride in water, then add ammonia water dropwise under stirring, and stop adding ammonia water dropwise when the system pH is 9-10 to obtain a mixed solution;
[0013] The mixed solution is subjected to a hydrothermal reaction treatment, and then the precipitate is taken out and washed, dried and ground to obtain the monoclinic and tetragonal mixed zirconium oxide precursor.
[0014] Furthermore, the working condition parameters of the hydrothermal reaction treatment include: temperature of 110 to 140° C. and time of 6 to 36 hours.
[0015] Furthermore, the weight ratio of the zirconium oxide precursor, the pseudo-boehmite and the sulfuric acid solution is (6-7):(2-3):(10-50); and the molar concentration of the sulfuric acid solution is 0.1-2.0 mol / L.
[0016] Furthermore, the weight ratio of the carrier precursor, the sesbania powder, the silica sol, the acid and the water is 1:(0.01-0.05):(0.01-0.03):(0.02-0.05):(0.2-0.3).
[0017] Furthermore, the working condition parameters of the first roasting include: the working condition parameters of the first roasting include: temperature of 500-700°C, time of 2-4 hours; the working condition parameters of the second roasting include: temperature of 500-650°C, time of 2-4 hours; the working condition parameters of the third roasting include: temperature of 450-600°C, time of 2-4 hours.
[0018] Furthermore, the noble metal active component is selected from at least one of platinum and palladium.
[0019] In a second aspect, the present invention provides a solid super acid isomerization catalyst, wherein the solid super acid isomerization catalyst is prepared by the preparation method of the solid super acid isomerization catalyst described in any one of the first aspects.
[0020] In a third aspect, the present invention provides use of the solid superacid isomerization catalyst described in any one of the second aspects in the isomerization reaction of normal alkanes.
[0021] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0022] The embodiment of the present invention provides a solid superacid isomerization catalyst and a preparation method and application thereof. The preparation method of the solid superacid isomerization catalyst provided by the present invention is used for the isomerization reaction of normal alkanes, has a simple process flow, low equipment requirements, has excellent catalyst activity, excellent selectivity and stability, and solves the problem of insufficient activity of existing solid superacid catalysts. Specifically:
[0023] 1. Compared with traditional isomerization catalysts, the superacid isomerization catalyst provided by the present invention has high catalytic activity, good selectivity, excellent stability, high strength, appropriate bulk ratio, and wide applicability.
[0024] 2. The carrier is prepared using a monoclinic and tetragonal mixed zirconia precursor as a raw material, which has a better sulfur fixation effect, can increase the sulfur content of the carrier, has a simple process, and is suitable for actual factory production.
[0025] 3. The product of the present invention has low process energy consumption, produces less by-product waste during the preparation process, has an extrusion molding method and a complete process, and can be quickly industrialized. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 The present invention provides a flow chart of a method for preparing a solid superacid isomerization catalyst according to an embodiment of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0031] In a first aspect, the present invention provides a method for preparing a solid superacid isomerization catalyst, such as Figure 1 As shown, the preparation method comprises the following steps:
[0032] A monoclinic and tetragonal mixed zirconium oxide precursor is obtained;
[0033] The zirconium oxide precursor and pseudo-boehmite are mixed, and then a sulfuric acid solution is added for soaking, filtering, drying, grinding and first calcining to obtain a carrier precursor;
[0034] The carrier precursor, sesbania powder, silica sol, acid solution and water are kneaded and then extruded, and then placed at room temperature, dried and second calcined to obtain a catalyst carrier;
[0035] The noble metal active component is impregnated on the catalyst carrier by adopting an equal volume impregnation method, and then aging and a third calcination are performed to obtain the solid superacid isomerization catalyst.
[0036] The preparation method of the solid superacid isomerization catalyst provided by the present invention is used for the isomerization reaction of normal alkanes, has a simple process flow, low equipment requirements, and has excellent catalyst activity, excellent selectivity and stability, solving the problem of insufficient activity of existing solid superacid catalysts. Specifically:
[0037] 1. Compared with traditional isomerization catalysts, the superacid isomerization catalyst provided by the present invention has high catalytic activity, good selectivity, excellent stability, high strength, appropriate bulk ratio, and wide applicability.
[0038] 2. The carrier is prepared using a monoclinic and tetragonal mixed zirconia precursor as a raw material, which has a better sulfur fixation effect, can increase the sulfur content of the carrier, has a simple process, and is suitable for actual factory production.
[0039] 3. The product of the present invention has low process energy consumption, produces less by-product waste during the preparation process, has an extrusion molding method and a complete process, and can be quickly industrialized.
[0040] In some specific embodiments, the step of obtaining a monoclinic and tetragonal mixed zirconium oxide precursor comprises the following process:
[0041] Dissolve zirconium oxychloride in water, then add ammonia water dropwise under stirring, and stop adding ammonia water dropwise when the system pH is 9-10 to obtain a mixed solution;
[0042] The mixed solution is subjected to a hydrothermal reaction treatment, and then the precipitate is taken out and washed, dried and ground to obtain the monoclinic and tetragonal mixed zirconium oxide precursor.
[0043] In some specific embodiments, the working condition parameters of the hydrothermal reaction treatment include: a temperature of 110 to 140° C. and a time of 6 to 36 hours.
[0044] In some specific embodiments, the weight ratio of the zirconium oxide precursor, the pseudo-boehmite and the sulfuric acid solution is (6-7):(2-3):(10-50); the molar concentration of the sulfuric acid solution is 0.1-2.0 mol / L.
[0045] In some specific embodiments, the weight ratio of the carrier precursor, the sesbania powder, the silica sol, the acid and the water is 1:(0.01-0.05):(0.01-0.03):(0.02-0.05):(0.2-0.3).
[0046] In some specific embodiments, the working condition parameters of the first roasting include: temperature of 500-700°C, time of 2-4 hours; the working condition parameters of the second roasting include: temperature of 500-650°C, time of 2-4 hours; the working condition parameters of the third roasting include: temperature of 450-600°C, time of 2-4 hours.
[0047] In some specific embodiments, the noble metal active component is selected from at least one of platinum and palladium.
[0048] In a second aspect, the present invention provides a solid super acid isomerization catalyst, wherein the solid super acid isomerization catalyst is prepared by the preparation method of the solid super acid isomerization catalyst described in any one of the first aspects.
[0049] In a third aspect, the present invention provides use of the solid superacid isomerization catalyst described in any one of the second aspects in the isomerization reaction of normal alkanes.
[0050] It should be noted that the components and raw materials involved in the solid superacid isomerization catalyst and its preparation method and application provided in the embodiments of the present invention can directly use commercially available products unless otherwise specified or described. At the same time, the operation steps involved can be performed with reference to the prior art or using existing equipment unless otherwise specified.
[0051] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0052] Example 1
[0053] This example provides a solid superacid isomerization catalyst, and the preparation method thereof comprises the following steps:
[0054] Weigh 4000g zirconium oxychloride and 5500g deionized water, add to the reactor and stir until the zirconium oxychloride is completely dissolved, keep stirring and add 3000g ammonia water dropwise, the ammonia concentration is 25-28%. After the pH of the mixed solution reaches 9-10, seal the reactor and heat to 125℃. After reacting for 24 hours, take out the precipitate and wash until there is no Cl - , dried at 110°C and then ground to obtain a zirconium oxide precursor mixed with monoclinic and tetragonal phases.
[0055] 700 g of the above-mentioned zirconium oxide precursor and 300 g of pseudo-boehmite were mixed, 2 kg of 1 mol / L sulfuric acid solution was added, and the mixture was immersed in a stirring state for 2 hours, and then filtered, dried, ground, and calcined at 600° C. for 3 hours to obtain a carrier precursor.
[0056] The above carrier precursor was placed in a kneader, and 30 g of sesbania powder, 20 g of silica sol, 30 g of nitric acid, 20 g of acetic acid and 250 g of deionized water were added. After fully kneading, it was extruded, placed at room temperature for 12 hours, dried at 110°C for 12 hours, and calcined at 650°C for 3 hours to obtain a catalyst carrier. 500 g of the carrier was weighed, and chloroplatinic acid solution was prepared for equal volume impregnation. After fully impregnating, it was aged for 12 hours, dried, and calcined at 500°C for 3 hours to obtain a solid superacid isomerization catalyst, which was recorded as sample A.
[0057] Example 2
[0058] This example provides a solid superacid isomerization catalyst, and the preparation method thereof comprises the following steps:
[0059] Weigh 4000g of zirconium oxychloride and 5500g of deionized water, add them into a reactor and stir until the zirconium oxychloride is completely dissolved, and add 3000g of ammonia water dropwise while maintaining the stirring state, with the ammonia water concentration being 25-28%. After the pH of the mixed solution reaches 9-10, seal the reactor and heat it to 130°C, react for 24 hours, take out the precipitate, filter and wash it twice, dry it at 110°C, and grind it to obtain a zirconium oxide precursor mixed with monoclinic and tetragonal phases.
[0060] 640 g of the above-mentioned zirconium oxide precursor and 360 g of pseudo-boehmite were mixed, 2 kg of 0.5 mol / L sulfuric acid solution was added, and the mixture was immersed in stirring for 2 hours, and then filtered, dried, ground, and calcined at 600° C. for 3 hours to obtain a carrier precursor.
[0061] The above carrier precursor was placed in a kneader, and 50 g of sesbania powder, 20 g of silica sol, 25 g of nitric acid, 25 g of acetic acid and 260 g of deionized water were added. After fully kneading, it was extruded, placed at room temperature for 12 hours, dried at 110°C for 12 hours, and calcined at 650°C for 3 hours to obtain a catalyst carrier. 500 g of the carrier was weighed, and chloroplatinic acid solution was prepared for equal volume impregnation. After fully impregnating, it was aged for 12 hours, dried, and calcined at 500°C for 3 hours to obtain a solid superacid isomerization catalyst, which was recorded as sample B.
[0062] Example 3
[0063] This example provides a solid superacid isomerization catalyst, and the preparation method thereof comprises the following steps:
[0064] Weigh 4000g of zirconium oxychloride and 5500g of deionized water, add them into a reactor and stir until the zirconium oxychloride is completely dissolved, and add 3000g of ammonia water dropwise while maintaining the stirring state, with the ammonia water concentration being 25-28%. After the pH of the mixed solution reaches 9-10, seal the reactor and heat it to 125°C, react for 24 hours, take out the precipitate, filter and wash it 3 times, dry it at 110°C, and grind it to obtain a zirconium oxide precursor mixed with monoclinic and tetragonal phases.
[0065] 700 g of the above zirconium oxide precursor and 300 g of pseudo-boehmite were mixed, 2 kg of 1 mol / L sulfuric acid solution was added, and the mixture was immersed in stirring state for 2 hours, and then filtered, dried, ground, and calcined at 600° C. for 3 hours to obtain a carrier precursor.
[0066] The above carrier precursor was placed in a kneader, and 30 g of sesbania powder, 25 g of silica sol, 50 g of hydrochloric acid and 270 g of deionized water were added. After fully kneading, it was extruded, placed at room temperature for 12 hours, dried at 110°C for 12 hours, and calcined at 650°C for 3 hours to obtain a catalyst carrier. 500 g of the carrier was weighed, and chloroplatinic acid solution was prepared for equal volume impregnation. After fully impregnating, it was aged for 12 hours, dried, and calcined at 500°C for 3 hours to obtain a solid superacid isomerization catalyst, which was recorded as sample C.
[0067] Example 4
[0068] This example provides a solid superacid isomerization catalyst, and the preparation method thereof comprises the following steps:
[0069] Weigh 4000g of zirconium oxychloride and 5500g of deionized water, add to a reactor and stir until the zirconium oxychloride is completely dissolved, and add 3000g of ammonia water dropwise while maintaining the stirring state, with the ammonia water concentration being 25-28%. After the pH of the mixed solution reaches 9-10, seal the reactor and heat to 125°C, react for 24 hours, take out the precipitate, filter and wash it twice, dry it at 110°C, and grind it to obtain a zirconium oxide precursor mixed with monoclinic and tetragonal phases.
[0070] 700 g of the above zirconium oxide precursor and 300 g of pseudo-boehmite were mixed, 2 kg of 1 mol / L sulfuric acid solution was added, and the mixture was immersed in stirring state for 2 hours, and then filtered, dried, ground, and calcined at 600° C. for 3 hours to obtain a carrier precursor.
[0071] The above carrier precursor was placed in a kneader, and 30 g of sesbania powder, 25 g of silica sol, 25 g of nitric acid, 25 g of acetic acid and 260 g of deionized water were added. After fully kneading, it was extruded, placed at room temperature for 12 hours, dried at 110°C for 12 hours, and calcined at 650°C for 3 hours to obtain a catalyst carrier. 500 g of the carrier was weighed, and chloroplatinic acid solution was prepared for equal volume impregnation. After fully impregnating, it was aged for 12 hours, dried, and calcined at 500°C for 3 hours to obtain a solid superacid isomerization catalyst, which was recorded as sample D.
[0072] Comparative Example 1
[0073] This example provides a solid superacid isomerization catalyst and a preparation method thereof, which differs from Example 1 only in that: there is no 24-hour 125°C hydrothermal reaction during the preparation of the zirconium oxide precursor (i.e., no conventional zirconium oxide precursor), and the other preparation processes are the same as Example 1, recorded as Comparative A.
[0074] Test Case
[0075] The present invention uses a laboratory customized micro-evaluation device for evaluation. The catalyst particle size is 20-60 mesh, the loading mass is 5g, the reaction temperature is 140-250°C, the reaction pressure is 1.0-3.0MPa, and the mass space velocity is 0.5-3.0h -1 , the hydrogen-to-oil molar ratio is 0.5-3.0. The catalyst needs to be air activated and hydrogen reduced before activity evaluation. Heat to 400-500°C at a heating rate of 3-10°C / min and keep constant for 2-4 hours, and introduce dry air for activation. After activation, cool to 250°C, purge with nitrogen for 0.5-2 hours, and after purging, introduce hydrogen for catalyst reduction, maintain the temperature at 250°C, and reduce for 1-4 hours. In addition, no activation and reduction treatment is performed before evaluation, and the rest of the preparation process is the same as Example 1, recorded as Comparative B.
[0076] The physicochemical indicators of the catalyst are shown in Table 1, and the isomerization performance test data of the catalyst are shown in Table 2.
[0077] Table 1
[0078]
[0079]
[0080] Table 2 Performance evaluation of catalyst after continuous reaction for 100 hours
[0081]
[0082]
[0083] It can be seen from Table 1 and Table 2 above that the superacid catalyst prepared in the embodiment of the present invention has better isomerization catalytic reaction performance. After 100 hours of continuous reaction, it has better catalytic activity, high n-hexane conversion rate, good selectivity, excellent stability, and can be quickly industrialized.
[0084] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0085] In the present invention, in the absence of contrary instructions, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of the present invention, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0086] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a solid superacid isomerization catalyst, characterized in that: The preparation method comprises the following steps: A monoclinic and tetragonal mixed zirconium oxide precursor is obtained; The zirconium oxide precursor and pseudo-boehmite are mixed, and then a sulfuric acid solution is added for soaking, filtering, drying, grinding and first calcining to obtain a carrier precursor; The carrier precursor, sesbania powder, silica sol, acid solution and water are kneaded and then extruded, and then placed at room temperature, dried and second calcined to obtain a catalyst carrier; The noble metal active component is impregnated on the catalyst carrier by an equal volume impregnation method, and then aged and third calcined to obtain the solid superacid isomerization catalyst.
2. The method for preparing a solid superacid isomerization catalyst according to claim 1, characterized in that: The step of obtaining a monoclinic and tetragonal mixed zirconium oxide precursor comprises the following process: Dissolve zirconium oxychloride in water, then add ammonia water dropwise under stirring, and stop adding ammonia water when the system pH is 9-10 to obtain a mixed solution; The mixed solution is subjected to a hydrothermal reaction treatment, and then the precipitate is taken out and washed, dried and ground to obtain the monoclinic and tetragonal mixed zirconium oxide precursor.
3. The method for preparing a solid superacid isomerization catalyst according to claim 2, characterized in that: The working condition parameters of the hydrothermal reaction treatment include: temperature of 110 to 140° C. and time of 6 to 36 hours.
4. The method for preparing a solid superacid isomerization catalyst according to claim 1, characterized in that: The weight ratio of the zirconium oxide precursor, the pseudo-boehmite and the sulfuric acid solution is (6-7):(2-3):(10-50); the molar concentration of the sulfuric acid solution is 0.1-2.0 mol / L.
5. The method for preparing a solid superacid isomerization catalyst according to claim 1, characterized in that: The weight ratio of the carrier precursor, the sesbania powder, the silica sol, the acid and the water is 1:(0.01-0.05):(0.01-0.03):(0.02-0.05):(0.2-0.3).
6. The method for preparing a solid superacid isomerization catalyst according to claim 1, characterized in that: The working condition parameters of the first roasting include: temperature of 500-700°C and time of 2-4 hours; the working condition parameters of the second roasting include: temperature of 500-650°C and time of 2-4 hours; the working condition parameters of the third roasting include: temperature of 450-600°C and time of 2-4 hours.
7. The method for preparing a solid superacid isomerization catalyst according to claim 1, characterized in that: The noble metal active component is selected from at least one of platinum and palladium.
8. A solid superacid isomerization catalyst, characterized in that: The solid superacid isomerization catalyst is prepared by the preparation method of the solid superacid isomerization catalyst according to any one of claims 1 to 7.
9. Use of the solid superacid isomerization catalyst according to claim 8 in the isomerization reaction of normal alkanes.
Citation Information
Patent Citations
Method of manufacturing high isomerization active solid super acidic catalyst
CN101108355A
N-butane isomerization catalyst and preparation method thereof
CN107051420A
Method for preparation of superstrong acid of carried oxide system
CN1094995A
Light alkane isomerization catalyst and preparation method thereof
CN110605125A
Isomerization catalyst as well as preparation method and application thereof
CN113289673A
Cited By
Solid superacid catalyst as well as preparation method and application thereof
CN122499804A