High-resistance laminated iron and manufacturing method thereof
By using the laminated thermal lamination technology of a low-roughness substrate and a three-layer structure polyester film in the coated iron, the problem of insufficient corrosion resistance of the coated iron in the existing technology has been solved, and it has been achieved under high-temperature sterilization conditions. High salt resistance and sulfur resistance meet the high resistance requirements of food metal packaging.
Patent Information
- Application Number
- CN202310457422.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing coated iron has deficiencies in corrosion resistance, especially in salty or sulfur-containing environments, and the existing technology does not fully pay attention to the impact of the substrate surface and the interface between the film and the substrate on the resistance.
A low-roughness substrate (0.15~0.35μm) is used and treated with oil, and is combined with a three-layer polyester film for thermal lamination. The thermal lamination layer, middle layer and barrier layer are made of modified copolymer polyester, uniform Made of polyester and non-modified homopolyester, the interface adhesion performance and resistance are improved through thermal lamination technology.
After the can is formed, it can significantly improve the salt resistance and sulfur resistance under high-temperature sterilization conditions. It is suitable for the field of food metal packaging with high resistance requirements and avoids problems of interface adhesion and corrosion resistance.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a composite material and a manufacturing method thereof, in particular to a coated iron and a manufacturing method thereof. Background Art
[0002] Laminated iron generally refers to a composite material obtained by directly laminating a high-molecular polyester film on a steel substrate by heating and melting. It can be used as both a can body and a can cover material, and can be applied to food cans, beverage cans, ordinary covers, easy-open covers, etc. Food canning application is one of the important development directions of laminated iron. Among them, when the content of the food filling is mainly meat, or differentiated foods such as pickled garlic and crabs, higher resistance requirements are placed on the can body. The resistance of laminated iron is closely related to the type and structure of the surface film, as well as the interface performance between the film and the substrate.
[0003] A Chinese patent document with publication number CN 101646712A and publication date February 10, 2010, entitled "Polyester resin for metal plate coating and preparation method thereof" provides a polyester resin for metal plate coating, which is a polyester resin for metal plate coating formed by an acid component mainly composed of terephthalic acid and containing 1 to 15 mol% of isophthalic acid and 2 to 10 mol% of dimer acid and an alcohol component mainly composed of ethylene glycol. The polyester resin is characterized by excellent impact resistance and processing adhesion, but its corrosion resistance is evaluated by using a distilled water simulation liquid at 125 degrees for 30 minutes, and does not reflect resistance to simulated liquids containing salt or sulfur.
[0004] In addition, the current performance of coated iron focuses on its adhesion performance, and its corrosion resistance is usually improved by designing modified polymer films. However, as a composite material, the existing technology does not focus on the influence of the substrate surface and the interface state between the film and the substrate on the product resistance.
[0005] Based on this, it is hoped to provide a coated iron and a method for manufacturing the same that can meet the demand for high resistance. Summary of the invention
[0006] One of the purposes of the present invention is to provide a highly resistant coated iron, which adopts a low-roughness substrate and then heat-coats a polyester film with a multi-layer structure on the substrate through lamination, so as to form a coated iron product which has high resistance to high-temperature sterilization, especially salt resistance and sulfur resistance, after being deformed during canning.
[0007] In order to achieve the above object, the present invention proposes a high-resistance coated iron, which includes a substrate and a polyester film coated on the surface of the substrate, wherein:
[0008] The surface roughness of the substrate is 0.15 to 0.35 μm, and the surface of the substrate is treated with oil;
[0009] The polyester film comprises a heat-bonding layer, an intermediate layer and a barrier layer in order from top to bottom in the thickness direction, wherein the heat-bonding layer is composed of modified copolyester, the intermediate layer is a mixture of modified copolyester and homopolyester, and the barrier layer is composed of unmodified homopolyester.
[0010] The present invention adopts a substrate with low surface roughness and a three-layer polyester film, and laminates the polyester film on the substrate by heat lamination, thereby obtaining high interface adhesion performance. After canning and forming, high-temperature sterilization can greatly improve its resistance, and the present invention is suitable for the field of food metal packaging that has high resistance requirements for the filled contents.
[0011] Among them, the low surface roughness of 0.15 to 0.35 μm is an important surface quality indicator of the substrate, which is closely related to the surface performance of the coated iron and is related to the adhesion and corrosion resistance of the coated iron described in the present invention.
[0012] The three-layer polyester film has an upper layer that can well meet the thermal lamination between the substrate and the film, has excellent adhesion properties, and can meet the processing and forming requirements. At the same time, the lower layer can provide good barrier properties and meet the requirements of high resistance. The middle layer is a transition layer, which avoids structural damage to the non-laminated layer due to heat and can prevent delamination during the deformation process of the film.
[0013] Furthermore, in the high-resistance coated iron described in the present invention, the substrate is a chrome-plated plate.
[0014] Of course, in other embodiments, the substrate may also be other plates, such as a tin-plated plate.
[0015] Furthermore, in the high-resistance coated iron of the present invention, the surface of the substrate is coated with oil, and the surface oil coating amount of the substrate is 1.5 to 3.5 mg / m 2 .
[0016] Generally speaking, the main purpose of oiling the substrate is to prevent rust and lubricate and prevent friction. However, the inventors of this case found that too much oiling can easily have a negative impact on the interface adhesion performance after coating. In normal use, the coated iron will be deformed after canning, which will cause interface adhesion and affect its corrosion resistance. Based on this, the present invention reduces the amount of oil applied on the substrate surface to 1.5-3.5 mg / m 2 , to ensure better interface adhesion performance.
[0017] Furthermore, in the high-resistance coated iron of the present invention, the type of oil coating is selected from at least one of the following: dioctyl sebacate (DOS), cottonseed oil (CSO), and acetyl tri-n-butyl citrate (ATBC).
[0018] Furthermore, in the high-resistance coated iron of the present invention, the melting point of the modified copolyester is 220-232°C.
[0019] Furthermore, in the high-resistance coated iron of the present invention, the modified copolymer polyester is obtained by copolymerizing polyester with isophthalic acid or aliphatic diol.
[0020] Furthermore, in the high-resistance coated iron described in the present invention, the aliphatic diol is selected from at least one of the following: propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, and 1 / 4-cyclohexanedimethanol.
[0021] Furthermore, in the high-resistance coated iron of the present invention, the aliphatic diol is selected from: neopentyl glycol and / or 1 / 4-cyclohexanedimethanol.
[0022] Furthermore, in the high-resistance coated iron described in the present invention, the non-modified homopolymer polyester is ethylene terephthalate.
[0023] Furthermore, in the high-resistance coated iron of the present invention, the melting point of the non-modified homopolyester is 250-260°C.
[0024] Furthermore, in the high-resistance coated iron of the present invention, the mass percentage of the modified copolyester in the intermediate layer is 20% to 80%.
[0025] Furthermore, the mass percentage of the modified copolyester in the middle layer is 30% to 70%.
[0026] Furthermore, in the high-resistance coated iron of the present invention, the thickness of the polyester film is 20 to 35 μm.
[0027] Furthermore, the polyester film has a thickness of 25 to 30 μm.
[0028] Another object of the present invention is to provide a method for manufacturing high-resistance coated iron, by which a highly resistant coated iron product can be produced.
[0029] Based on the above purpose, the present invention also provides a method for manufacturing the high-resistance coated iron as described above, which comprises the steps of:
[0030] Performing heating pretreatment on the substrate;
[0031] Film thermal lamination;
[0032] Cool and squeeze dry.
[0033] Furthermore, in the heating pretreatment step of the manufacturing method of the present invention, the substrate with the surface coated with oil is heated to 150-180°C.
[0034] Heating the substrate to a temperature of 150-180°C is conducive to the volatilization of the oil on the substrate surface, further reducing the amount of oil on the substrate surface. After the oil evaporates, the induction heating roller can be used to make the substrate temperature reach the target coating temperature and keep it stable.
[0035] Furthermore, in the manufacturing method of the present invention, in the film thermal lamination step, the lamination speed is controlled to be 60-120 m / min.
[0036] Furthermore, in the cooling and squeezing step of the manufacturing method described in the present invention, the coated iron is first cooled to below 80° C. by spraying water, then water quenched in a water quenching tank, and then squeezed by a squeezing roller.
[0037] The high-resistance coated iron of the present invention has the following advantages and beneficial effects:
[0038] The present invention adopts a low-roughness, low-oil substrate, pre-treats the surface by heating to remove oil, and then heat-coats a three-layer polyester film on the substrate by lamination to form a coated iron product that can meet high resistance requirements, especially salt resistance and sulfur resistance.
[0039] The three-layer polyester film used in the present invention has an upper layer that can well meet the thermal bonding between the substrate and the film, a lower layer that can provide good barrier properties and meet the requirements of high resistance, and a middle layer that is a transition layer that can prevent delamination during film deformation.
[0040] In some preferred embodiments of the present invention, the roughness Ra value range is 0.15 to 0.35 μm, and the surface oil coating amount is 1.5 to 3.5 mg / m 2 The substrate can effectively improve the interface adhesion performance of the coated iron and meet the requirements of high resistance after canning deformation.
[0041] After the coated iron of the present invention is canned, it is sterilized at 121°C for 60 min using 3% NaCl solution and cysteine simulation solution. The inner wall has no abnormal phenomena such as whitening, white bubbles, and sulfide spots, and can meet the high resistance requirements of foods such as fish and meat. DETAILED DESCRIPTION
[0042] The high-resistance coated iron and the method for manufacturing the same described in the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an undue limitation on the technical solution of the present invention.
[0043] Examples 1-6 and Comparative Examples 1-2
[0044] In the present invention, the coated iron of Examples 1-6 is prepared by the following steps:
[0045] (1) Using an induction heater to pre-heat the chrome-plated or tin-plated substrate: the surface roughness Ra of the substrate is 0.15-0.35 μm, and the amount of oil applied on the substrate surface is 1.5-3.5 mg / m 2 In order to do this, the substrate is heated to a temperature of 150 to 180°C.
[0046] (2) Film thermal lamination: A polyester film having a three-layer structure is thermally laminated on a substrate by a laminating roller at a laminating speed of 60 to 120 m / min. The polyester film comprises a thermal laminating layer, an intermediate layer and a barrier layer in the thickness direction from top to bottom, wherein the thermal laminating layer is composed of a modified copolyester, the intermediate layer is a mixture of a modified copolyester and a homopolyester, and the barrier layer is composed of a non-modified homopolyester, and the non-modified homopolyester is ethylene terephthalate.
[0047] In some embodiments, the modified copolyester is obtained by copolymerizing polyester with isophthalic acid or aliphatic diol, wherein the aliphatic diol can be selected from: neopentyl glycol and / or 1 / 4-cyclohexanedimethanol.
[0048] It should be noted that, although not listed in the following embodiments, the aliphatic diol can also be selected from at least one of the following: propylene glycol, butanediol, pentanediol, and hexanediol.
[0049] In some embodiments, the melting point of the modified copolyester may be 220-232° C. The melting point of the unmodified homopolyester is 250-260° C. The mass percentage of the modified copolyester in the middle layer is 20%-80%.
[0050] In some embodiments, the polyester film has a thickness of 20 to 35 μm.
[0051] (3) Cooling and squeezing: First, the coated iron is cooled to below 80°C by spraying water, then quenched in a water quenching tank, and then squeezed dry by a squeezing roller.
[0052] Tables 1 and 2 list the specific process parameters of Examples 1-6 of the present invention and Comparative Examples 1-2.
[0053] Table 1.
[0054] Substrate Type Substrate Ra(μm) <![CDATA[Coating oil amount on substrate (mg / m 2 )]]> Oil type Preheating temperature (℃) Example 1 Chrome-plated substrate 0.35 3.5 DOS 180 Example 2 Chrome-plated substrate 0.35 1.5 DOS 180 Example 3 Chrome-plated substrate 0.30 3.5 DOS 170 Example 4 Chrome-plated substrate 0.25 1.5 DOS 170 Example 5 Chrome-plated substrate 0.20 2.0 ATBC 170 Example 6 Chrome-plated substrate 0.15 1.5 CSO 150 Comparative Example 1 Chrome-plated substrate 0.40 1.5 DOS 180 Comparative Example 2 Chrome-plated substrate 0.40 5 DOS 180
[0055] Table 2.
[0056]
[0057]
[0058] The coated iron of Examples 1-6 and the comparative coated iron of Comparative Examples 1-2 finally prepared by the above process of the present invention were sampled respectively, and the interface adhesion performance, salt resistance performance and sulfur resistance test were performed on the samples of each Example and Comparative Example, and the test results of the above test were listed in the following Table 3. The test methods of interface adhesion performance, salt resistance performance and sulfur resistance are as follows:
[0059] Interface adhesion performance: Adopt the cross-grid cupping tape stripping method to measure the adhesion after deformation. Take a 10cm×10cm coated iron, and draw a "well" grid on the flat plate with an interval of 5mm. After cutting through the film (be careful not to scratch the substrate), use the cupping deformation to keep the highest point of the cupping in the middle area of the "well". Then put the sample into the pressure steam sterilizer and use 121℃*60min high temperature sterilization treatment. After taking out the sample, observe whether there is film peeling at the cross-grid, especially at the intersection of the "well" grid, so as to evaluate the film adhesion performance.
[0060] Salt resistance: After the coated iron is canned (can type 538), the coated can is filled with 3% NaCl solution, capped and steamed at 121°C for 30 minutes, and after cooling, the sample is taken out to observe whether there are abnormal phenomena such as whitening, bubbling, film shedding, etc. on the surface. This is used to evaluate the salt resistance of the coated metal plate.
[0061] Anti-sulfur performance: After the coated iron is flushed into a can (can type 538), the coated can is filled with cysteine simulation solution (anti-sulfur test reagent: 0.56g L-cysteine, 3.6g potassium dihydrogen phosphate and 7.2g disodium hydrogen phosphate are dissolved to a volume of 1000mL), and then capped and steamed at 121℃ for 60min. After cooling, the sample is taken out to observe whether there are abnormal phenomena such as whitening, sulfide spots, film shedding, etc. on the surface. This is used to evaluate the anti-sulfur performance of the coated metal plate.
[0062] Table 3 lists the relevant performance test results of the coated iron of Examples 1-6 and Comparative Examples 1-2.
[0063] Table 3.
[0064] serial number Adhesion performance Anti-sulfur performance Salt resistance Example 1 ◎ ○ ○ Example 2 ◎ ○ ○ Example 3 ◎ ◎ ◎ Example 4 ◎ ◎ ◎ Example 5 ○ ◎ ◎ Example 6 ○ ◎ ◎ Comparative Example 1 ○ △ △ Comparative Example 2 △ ╳ ╳
[0065] Note: In the above Table 3, “╳” indicates that the corresponding performance is unqualified; “△” indicates that the corresponding performance is qualified; “○” indicates that the corresponding performance is good; and “◎” indicates that the corresponding performance is excellent. The evaluation criteria are shown in Table 4 below.
[0066] Table 4.
[0067] Rating Adhesion performance Anti-sulfur performance Salt resistance excellent No peeling No whitening No white bubbles, no discoloration good Stripping length ≤ 0.5mm The bottom of the tank is slightly white No white foam tank bottom, slight discoloration of tank body qualified Stripping length ≤1.0mm The bottom of the can is slightly white There are 1-2 white bubbles on the can body Failure Stripping length>1.0mm Bubbling and film removal on the bottom and body of the tank There are >2 white bubbles on the can
[0068] It can be seen from Table 3 that Examples 1-6 of the present invention have excellent surface adhesion performance, and also have excellent salt resistance and sulfur resistance.
[0069] After the coated iron of the present invention is canned, it is sterilized at 121°C for 60 min using 3% NaCl solution and cysteine simulation solution. The inner wall has no abnormal phenomena such as whitening, white bubbles, and sulfide spots, and can meet the high resistance requirements of foods such as fish and meat.
[0070] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0071] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.
Claims
1. A high-resistance coated iron, comprising a substrate and a polyester film coated on the surface of the substrate, Features: The surface roughness of the substrate is 0.15 to 0.35 μm; The polyester film comprises a heat-bonding layer, an intermediate layer and a barrier layer in order from top to bottom in the thickness direction, wherein the heat-bonding layer is composed of modified copolyester, the intermediate layer is a mixture of modified copolyester and homopolyester, and the barrier layer is composed of unmodified homopolyester.
2. The high-resistance coated iron according to claim 1, It is characterized in that The substrate is a chrome-plated plate.
3. The high-resistance coated iron according to claim 1, It is characterized in that The surface of the substrate is coated with oil, and the amount of oil applied to the surface of the substrate is 1.5 to 3.5 mg / m 2 .
4. The high-resistance coated iron according to claim 3, It is characterized in that The type of the coating oil is selected from at least one of the following: dioctyl sebaceate, cottonseed oil, and tri-n-butyl acetyl citrate.
5. The high-resistance coated iron according to claim 1, It is characterized in that The melting point of the modified copolyester is 220-232°C.
6. The high-resistance coated iron according to claim 1, It is characterized in that The modified copolymer polyester is obtained by copolymerizing and modifying polyester with isophthalic acid or aliphatic diol.
7. The high-resistance coated iron according to claim 6, It is characterized in that The aliphatic diol is selected from at least one of the following: propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, and 1 / 4-cyclohexanedimethanol.
8. The high-resistance coated iron according to claim 7, It is characterized in that The aliphatic diol is selected from: neopentyl glycol and / or 1 / 4-cyclohexanedimethanol.
9. The high-resistance coated iron according to claim 1, It is characterized in that The non-modified homopolymer polyester is ethylene terephthalate.
10. The high-resistance coated iron according to claim 1, It is characterized in that The melting point of the non-modified homopolyester is 250-260°C.
11. The high-resistance coated iron according to claim 1, It is characterized in that The mass percentage of the modified copolyester in the middle layer is 20% to 80%.
12. The high-resistance coated iron according to claim 1, It is characterized in that The polyester film has a thickness of 20 to 35 μm.
13. The method for producing high-resistance coated iron according to any one of claims 1 to 12, It is characterized in that Includes steps: Performing heating pretreatment on the substrate; Film thermal lamination; Cool and squeeze dry.
14. The manufacturing method according to claim 13, It is characterized in that In the heating pretreatment step, the substrate with the surface oiled is heated to 150-180°C.
15. The manufacturing method according to claim 13, It is characterized in that In the film thermal lamination step, the lamination speed is controlled to be 60-120 m / min.
16. The manufacturing method according to claim 13, It is characterized in that In the cooling and squeezing step, the coated iron is first cooled to below 80°C by spraying water, then water quenched in a water quenching tank, and then squeezed by a squeezing roller.
Citation Information
Patent Citations
Iron coating film and coated iron adopting same
CN105619982A
Laminated steel having extremely low interface gas bubble rate, and manufacturing method thereof
CN109910402A
Preparation method and film coated metal plate of single-layer copolymerized polyester iron-coated film
CN110920169A
Electrotinned steel plate and manufacturing method thereof
CN115961317A