Method for extracting niobium and tantalum from titanium white waste acid

By using a mixed solution of sulfuric acid and HF in titanium dioxide waste acid and a multi-step extraction process of bis(2-ethylhexyl)phosphite co-extractant, the problem of high-purity niobium pentoxide and niobium pentoxide in the existing technology is solved. Due to the difficulty in preparing tantalum, efficient and environmentally friendly extraction of niobium and tantalum has been achieved, improving product purity and resource utilization.

CN118854085APending Publication Date: 2024-10-29LOMON BILLIONS GRP CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411198494.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When existing technology extracts niobium and tantalum from titanium dioxide waste acid, it is difficult to obtain high-purity niobium pentoxide and tantalum pentoxide, and the use of hydrogen fluoride (HF) dissolution process is corrosive to equipment and the environment, and requires resource utilization. rate is low.

Method used

A mixture of sulfuric acid and HF is used to dissolve low-grade niobium slag, and bis(2-ethylhexyl) phosphite is used as a co-extraction agent to remove impurities through a multi-step extraction and washing process to improve the extraction rate of niobium and tantalum. Finally, high-purity niobium pentoxide and tantalum pentoxide are prepared through roasting.

Benefits of technology

It effectively reduces the consumption of HF, reduces the harm to equipment and the environment, and improves the purity of niobium and tantalum. The purity of the prepared niobium pentoxide and tantalum pentoxide can reach more than 99%, and the removal rate of Th and Sc is Reaching 98%, achieving efficient recycling of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854085A_ABST
    Figure CN118854085A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of niobium and tantalum recovery, in particular to a method for extracting niobium and tantalum from titanium white waste acid. Comprising the following steps: preparing low-grade niobium slag by utilizing the titanium white waste acid; a mixed solution of sulfuric acid and HF is adopted to dissolve the low-grade niobium slag, and a leaching solution is obtained; carrying out first extraction, washing, first reverse extraction and impurity removal on the leachate to obtain impurity-removed niobium-enriched reverse extraction liquid, and carrying out synergistic extraction by adopting a synergistic extraction agent bis (2-ethylhexyl) phosphite and a main extraction agent in the first extraction; carrying out tantalum extraction on the niobium-rich strip liquor through second extraction to obtain a tantalum-rich organic phase and raffinate, and carrying out second back extraction on the tantalum-rich organic phase to obtain tantalum-rich liquor; and respectively carrying out tantalum precipitation and niobium precipitation on the tantalum-rich liquid and the raffinate, carrying out solid-liquid separation, and respectively roasting the obtained precipitates to obtain the tantalum pentoxide and the niobium pentoxide. According to the method, the extraction rate of Nb is high, the product purity of niobium and tantalum oxides is high, the environmental pollution is small, and the wastewater treatment cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of niobium and tantalum recovery, and in particular to a method for extracting niobium and tantalum from titanium dioxide waste acid. Background Art

[0002] The existing preparation process of niobium oxide and tantalum oxide is to use niobium tantalum concentrate as raw material, use HF or KOH as leaching agent for acid leaching or alkaline leaching, then carry out tantalum-niobium co-extraction, and then use MIBK, TBP, cyclohexanone (CHN) and other extractants to separate Nb and Ta, and then precipitate Nb and Ta respectively, and obtain their oxides after roasting. However, the industry generally adopts ammonia precipitation to treat niobium liquid, which will produce a large amount of fluorine-containing and ammonia-containing wastewater. The precipitation wastewater is separated from ammonium fluoride by evaporation, and the wastewater treatment cost is high. In addition, the acid dissolution process in niobium tantalum concentrate adopts HF to dissolve, and HF is extremely corrosive and has high requirements on equipment. In addition, excessively high concentration of HF is also volatile, which also poses a threat to the environment and the health of workers.

[0003] Waste titanium dioxide acid contains a variety of valuable elements. If they can be extracted and recycled, it will not only avoid waste of resources but also be beneficial to environmental protection. However, when recovering niobium from waste titanium dioxide acid, the prior art usually obtains an enrichment of niobium and a variety of mixed metals such as scandium, titanium, and zirconium, but does not disclose how to use waste titanium dioxide acid to prepare high-purity niobium pentoxide and tantalum pentoxide. Therefore, it is of great significance to provide a clean and environmentally friendly method for extracting niobium and tantalum from waste titanium dioxide acid to prepare high-purity niobium pentoxide and tantalum pentoxide.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for extracting niobium and tantalum from titanium dioxide waste acid. The method of the present invention adopts a mixed solution of sulfuric acid and HF to dissolve low-grade niobium slag to effectively remove Th and Sc, and the extraction rate of niobium is improved by using a co-extractant. The purity of niobium pentoxide and tantalum pentoxide prepared by the method of the present invention is as high as more than 99%.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0007] A method for extracting niobium and tantalum from titanium dioxide waste acid comprises the following steps:

[0008] S1. Using titanium dioxide waste acid to prepare low-grade niobium slag;

[0009] S2. dissolving the low-grade niobium slag by a mixture of sulfuric acid and HF to obtain a leaching solution and a leaching slag;

[0010] S3. performing a first extraction on the leachate to obtain a niobium-rich organic phase, wherein the extractant of the first extraction comprises a main extractant and a co-extractant, and the co-extractant comprises bis(2-ethylhexyl)phosphite;

[0011] S4. washing the niobium-rich organic phase, performing a first stripping to obtain a niobium-rich stripping solution, and removing impurities from the niobium-rich stripping solution;

[0012] S5. extracting tantalum from the impurity-removed niobium-rich stripping solution by a second extraction to obtain a tantalum-rich organic phase and a raffinate, and performing a second stripping on the tantalum-rich organic phase to obtain a tantalum-rich solution;

[0013] S6. Precipitating tantalum from the tantalum-rich liquid, and roasting the resulting precipitate after solid-liquid separation to obtain tantalum pentoxide; Precipitating niobium from the raffinate, and roasting the resulting precipitate after solid-liquid separation to obtain niobium pentoxide.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The invention uses titanium dioxide waste acid as a raw material to extract niobium and tantalum. In the acid leaching stage of niobium extraction, pure HF is not used, but HF+sulfuric acid is used for dissolution, which can not only reduce the consumption of HF and reduce the harm to equipment, environment and workers; but also effectively remove Th and Sc, and the removal rate of Th and Sc can reach about 98%. In the extraction and niobium extraction stage, bis(2-ethylhexyl)phosphite is added as a co-extractant, which can increase the selectivity of the main extractant to niobium and effectively increase the extraction rate of Nb, and the purity of the finally obtained niobium pentoxide and tantalum pentoxide can reach more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 A schematic diagram of a process flow for extracting niobium and tantalum from waste titanium dioxide acid provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0018] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0019] like Figure 1 As shown, the present invention provides a method for extracting niobium and tantalum from titanium dioxide waste acid, comprising the following steps:

[0020] S1. Using titanium dioxide waste acid to prepare low-grade niobium slag;

[0021] S2. using a mixture of sulfuric acid and HF to dissolve low-grade niobium slag, remove Th and Sc, and obtain a leaching solution and a leaching slag, wherein the leaching slag is the precipitated Th and Sc;

[0022] S3. The leachate is subjected to a first extraction to obtain a niobium-rich organic phase, wherein the extractant of the first extraction comprises a main extractant and a co-extractant, wherein the co-extractant comprises bis(2-ethylhexyl)phosphite;

[0023] S4. washing the niobium-rich organic phase, performing a first stripping to obtain a niobium-rich stripping solution, and removing impurities from the niobium-rich stripping solution;

[0024] S5. extracting tantalum from the impurity-removed niobium-rich stripping solution by a second extraction to obtain a tantalum-rich organic phase and a raffinate (niobium-rich solution), and performing a second stripping on the tantalum-rich organic phase to obtain a tantalum-rich solution;

[0025] S6. Precipitating tantalum from the tantalum-rich liquid, and roasting the resulting precipitate after solid-liquid separation to obtain tantalum pentoxide; Precipitating niobium from the raffinate, and roasting the resulting precipitate after solid-liquid separation to obtain niobium pentoxide.

[0026] The invention uses titanium dioxide waste acid as a raw material to prepare low-grade niobium slag, and then performs acid leaching, extraction of niobium, niobium-tantalum separation, precipitation, and roasting on the low-grade niobium slag to prepare niobium pentoxide and tantalum pentoxide; HF+sulfuric acid is used for dissolution in the acid leaching stage, which can not only reduce the consumption of HF, but also reduce the harm to equipment, environment and workers; HF+sulfuric acid is used for dissolution to generate precipitation to effectively remove Th and Sc, and the precipitation rate of Th and Sc can reach about 98%, and the removal rate is high; in addition, in the extraction and extraction stage of niobium, bis(2-ethylhexyl)phosphite is added as a co-extractant, which can increase the selectivity of the main extractant to niobium and effectively increase the extraction rate of Nb, and the prepared niobium pentoxide and tantalum pentoxide have high purity, which can reach more than 99%.

[0027] In some specific embodiments of the present invention, in step S1, the method for preparing low-grade niobium slag comprises the following steps:

[0028] The titanium dioxide waste acid is subjected to a third extraction, and the obtained extract (loaded organic phase) is washed and stripped with sodium hydroxide to obtain a niobium-containing alkali cake; the niobium-containing alkali cake is subjected to an acid-based dissolution and impurity removal to obtain a low-grade niobium slag.

[0029] In some specific embodiments of the present invention, the extractant of the third extraction includes at least one of P204, P507, and P350; the above extractants can all extract niobium under acidic conditions, among which P204 has a large saturated extraction volume and a low price, and is the best choice.

[0030] In some specific embodiments of the present invention, the extraction phase ratio O / A of the third extraction is 1:15-1:25, for example, it can be any point value among 1:15, 1:18, 1:20, 1:22, 1:25 or a range value consisting of any two point values.

[0031] The niobium-containing alkali cake contains a large amount of Fe and Ti impurities. The purpose of using acid for optimal dissolution and impurity removal is mainly to remove Fe and Ti impurities. In some specific embodiments of the present invention, the pH of optimal dissolution and impurity removal is 0.5-3, for example, the pH can be any point value among 0.5, 1, 2, 3 or a range value consisting of any two point values.

[0032] In some specific embodiments of the present invention, in step S2, when the low-grade niobium slag is dissolved, the mass volume ratio of solid to liquid is 1:1-1:5, for example, it can be any point value among 1:1, 1:2, 1:3, 1:4, 1:5 or a range value consisting of any two point values, and the unit is g / mL.

[0033] In some specific embodiments of the present invention, in step S2, the concentration of sulfuric acid is 1-6 mol / L, for example, it can be any point value among 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, or a range value consisting of any two point values.

[0034] In some specific embodiments of the present invention, in step S2, the mass concentration of HF is 40%-50%, for example, it can be any point value among 40%, 42%, 45%, 48%, 50% or a range value consisting of any two point values.

[0035] In some specific embodiments of the present invention, in step S2, the volume ratio of sulfuric acid to HF is 2-4:1, for example, it can be any point value among 2:1, 3:1, 4:1 or a range value consisting of any two point values.

[0036] In the subsequent niobium extraction system, Nb is in the form of Nb(V) (NbF7 2- ) is extracted at a higher acidity. Too low sulfuric acid concentration will be lower than the optimal reaction acidity, while too low HF concentration will reduce the amount of F ions, thus affecting the extraction rate. Therefore, the ratio and concentration of sulfuric acid and HF need to be reasonably controlled.

[0037] In some specific embodiments of the present invention, in step S3, the main extractant includes at least one of TBP, MIBK, cyclohexanone, and 2-octanol.

[0038] The extractant of the third extraction in step S1 is mainly an extractant with a large saturated extraction amount, which can extract the valuable elements to the greatest extent, but the selectivity is relatively poor, and a variety of metals can be extracted; while the extractant in step S3 can selectively extract Nb through the synergistic effect of the main extractant and the co-extractant, which can effectively improve the extraction rate of Nb and thereby improve the product purity.

[0039] In some specific embodiments of the present invention, the extractant in step S3 also includes a solvent, for example, kerosene can be used as the solvent.

[0040] In some specific embodiments of the present invention, in step S3, the volume percentage of the main extractant to the extractant is 20%-50%, for example, it can be any point value among 20%, 30%, 40%, 50% or a range value consisting of any two point values.

[0041] If the concentration of the main extractant is too low, the extraction rate of Nb will be low. If the concentration of the main extractant is too high, it will affect the phase separation and cause the extraction efficiency to decrease. The concentration of the main extractant needs to be controlled within an appropriate range.

[0042] In some specific embodiments of the present invention, in step S3, the volume percentage of the co-extraction agent to the extractant is 3%-8%, for example, it can be any point value among 3%, 4%, 5%, 6%, 7%, 8% or a range value consisting of any two point values.

[0043] The synergistic extractant can improve the selectivity and extraction rate of the extractant for Nb. After adding the synergistic extractant, the overall extraction rate of Nb can be increased by 7-8%.

[0044] In some specific embodiments of the present invention, in step S3, the extraction phase ratio O / A of the first extraction is 1:1-3, for example, it can be any point value among 1:1, 1:2, 1:3 or a range value consisting of any two point values.

[0045] In some specific embodiments of the present invention, in step S4, the washing includes sulfuric acid washing, and the sulfuric acid concentration is 1.5-3 mol / L, for example, any point value among 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, or a range value consisting of any two point values.

[0046] In some specific embodiments of the present invention, in step S4, impurities are removed by adding alkali to adjust the pH to 3-5. For example, the pH can be any value among 3.2, 3.5, 4, 4.5, 5 or a range consisting of any two values. Typically but not limitatively, for example, the alkali used can be aqueous ammonia.

[0047] During the extraction of Nb in step S3, Sb(V) will also be converted into SbF6 - Therefore, Nb and Sb cannot be separated by extraction. The main purpose of adding alkali in the present invention is to remove Sb. When pH>3.2, Sb can be completely precipitated, so it can be removed by staged precipitation.

[0048] In some specific embodiments of the present invention, in step S5, the extractant for the second extraction includes MIBK and 2-octanol.

[0049] In some specific embodiments of the present invention, the second extractant further comprises a solvent, for example, the solvent may be kerosene.

[0050] In some preferred embodiments of the present invention, the second extractant is 20% MIBK, 5% 2-octanol and 75% solvent.

[0051] In some specific embodiments of the present invention, in step S5, the second extraction is a multi-stage countercurrent extraction, and the extraction ratio O / A is 1:8-12. For example, the extraction ratio O / A can be any point value among 1:8, 1:9, 1:10, 1:11, 1:12 or a range value consisting of any two point values.

[0052] In some specific embodiments of the present invention, the stripping agent of the first stripping and / or the second stripping is pure water.

[0053] In some specific embodiments of the present invention, in step S6, the precipitant for tantalum and / or niobium precipitation is boric acid. Using boric acid as a precipitant can effectively reduce the subsequent wastewater treatment cost.

[0054] In some specific embodiments of the present invention, the pH of the solution needs to be controlled to be less than 1 during the tantalum precipitation process.

[0055] In some specific embodiments of the present invention, the following steps are also included: adding potassium salt to the filtrate after tantalum and / or niobium precipitation, evaporating and concentrating to obtain potassium fluoroborate by-product, which can effectively realize resource recovery and effectively reduce the cost of the entire process.

[0056] The following is a detailed description of some embodiments of the present invention in conjunction with specific examples. The raw materials used in the examples can be purchased from the market unless otherwise specified.

[0057] Example 1

[0058] S1. Preparation of low-grade niobium slag using waste titanium dioxide acid: 25% P204 + 5% TBP + 70% 260# sulfonated kerosene was used as an extractant to extract the waste titanium dioxide acid by the chloride process at a ratio of O / A = 1:20, and the loaded organic phase was obtained after standing;

[0059] The loaded organic phase was extracted and washed with 6N hydrochloric acid at a phase ratio of O / A=7:10, and then the loaded organic phase was washed with 6N sulfuric acid at the same phase ratio, and then the loaded organic phase was stripped with 7M liquid alkali, the stripping phase ratio of O / A=5:9, and the stripping time was 6 minutes to obtain a niobium-containing alkali cake;

[0060] 500g of the above niobium-containing alkaline cake is added into 2L 10mol / L hydrochloric acid for dissolution, and the niobium-containing alkaline cake is continuously added to adjust the pH to 1±0.1. The above operation is repeated, the filter residue is dissolved again, and filtered to obtain a secondary acid-dissolved residue; the filter residue is dissolved again, the acidity is controlled at 0.1-0.2N, and filtered to obtain a low-grade niobium slag.

[0061] S2. HF+ sulfuric acid dissolution: 50g of the three-stage acid slag (low-grade niobium slag) was mixed with 150mL of 4.5mol / L sulfuric acid, and hydrofluoric acid with a mass concentration of 40% was added at 1 / 3 of the volume of sulfuric acid, and stirred at 50°C for 3h, and the leaching solution and leaching residue were obtained by filtration. The precipitation rate of Th was 98.72%, and the precipitation rate of Sc was 97.87%.

[0062] S3. First extraction: The above-mentioned leaching solution selected 30% TBP + 5% bis-(2-ethylhexyl) phosphite + 65% sulfonated kerosene as the extractant for single-stage extraction. The extraction ratio O / A = 1:3, the single-stage extraction rate of Nb was 52.7%.

[0063] S4. Washing, first stripping, impurity removal: 3 mol / L sulfuric acid was used to perform three-stage countercurrent washing and impurity removal on the organic phase at a phase ratio of O / A=1:1. Then, pure water was used to perform six-stage countercurrent stripping at a phase ratio of O / A=5:1 to obtain a niobium-rich stripping solution, and the pH was adjusted to between 3.2-4 with ammonia water, and filtered to remove Sb impurities therein.

[0064] S5. Second extraction and second stripping: 20% MIBK + 5% 2-octanol + 75% sulfonated kerosene are selected as the extractant, and the niobium-rich stripping solution is subjected to 12 levels of countercurrent stripping at a ratio of O / A = 1:10 to extract tantalum, to obtain a tantalum-rich organic phase and a raffinate, and the tantalum-rich organic phase is subjected to a second stripping with pure water, 5 levels of countercurrent stripping, and the stripping ratio O / A = 1:4 to obtain a tantalum-rich solution.

[0065] S6. Precipitating tantalum and niobium: adding boric acid to the tantalum-rich solution for precipitation, wherein the molar ratio of tantalum to boric acid in the tantalum-rich solution is 0.25, and the pH of the solution is controlled to be less than 1 at this stage, and the precipitate is calcined after filtering to obtain tantalum pentoxide;

[0066] Boric acid is added to the raffinate after tantalum extraction for precipitation, the molar ratio of niobium in the raffinate to boric acid is 0.25, and the precipitate is calcined after filtering to obtain niobium pentoxide.

[0067] The purity of niobium pentoxide and tantalum pentoxide prepared in this embodiment is both above 99%.

[0068] Example 2

[0069] The difference between Example 2 and Example 1 is that in step S3, the extractant is 20% TBP+5% bis-(2-ethylhexyl) phosphite+75% sulfonated kerosene, and the other conditions are the same as in Example 1.

[0070] Example 3

[0071] The difference between Example 3 and Example 1 is that in step S3, the extractant is 50% TBP+5% bis-(2-ethylhexyl) phosphite+45% sulfonated kerosene, and the other conditions are the same as in Example 1.

[0072] Example 4

[0073] The difference between Example 4 and Example 1 is that in step S3, the extractant is 30% TBP+3% bis-(2-ethylhexyl) phosphite+67% sulfonated kerosene, and the other conditions are the same as those in Example 1.

[0074] Example 5

[0075] The difference between Example 5 and Example 1 is that in step S3, the extractant is 30% TBP+8% bis-(2-ethylhexyl) phosphite+62% sulfonated kerosene, and the other conditions are the same as in Example 1.

[0076] Example 6

[0077] The difference between Example 6 and Example 1 is that the main extractant is MIBK, and the other conditions are the same as Example 1.

[0078] Example 7

[0079] The difference between Example 7 and Example 1 is that the main extractant is cyclohexanone, and the other conditions are the same as those of Example 1.

[0080] Example 8

[0081] The difference between Example 8 and Example 1 is that the main extractant is 2-octanol, and the other conditions are the same as Example 1.

[0082] Comparative Example 1

[0083] The difference between Comparative Example 1 and Example 1 is that in step S2, pure HF is used to dissolve the low-grade niobium slag, and the other conditions are the same as Example 1. The F content in the raffinate obtained by the first extraction is about 4-6 times that of Example 1, which increases the cost of wastewater treatment.

[0084] Comparative Example 2

[0085] The difference between Comparative Example 2 and Example 1 is that in step S3, bis-(2-ethylhexyl) phosphite is not added, the extractant is 30% TBP+70% sulfonated kerosene, and the other conditions are the same as in Example 1.

[0086] In each embodiment and each comparative example, the single-stage extraction rate of Nb in step S3 and the purity of the final niobium pentoxide and tantalum pentoxide are shown in Table 1.

[0087] Table 1

[0088]

[0089]

[0090] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for extracting niobium and tantalum from titanium dioxide waste acid, It is characterized in that The following steps are involved: S1. Using titanium dioxide waste acid to prepare low-grade niobium slag; S2. dissolving the low-grade niobium slag by a mixture of sulfuric acid and HF to obtain a leaching solution and leaching slag; S3. performing a first extraction on the leachate to obtain a niobium-rich organic phase, wherein the extractant of the first extraction comprises a main extractant and a co-extractant, and the co-extractant comprises bis(2-ethylhexyl)phosphite; S4. washing the niobium-rich organic phase, performing a first stripping to obtain a niobium-rich stripping solution, and removing impurities from the niobium-rich stripping solution; S5. extracting tantalum from the impurity-removed niobium-rich stripping solution by a second extraction to obtain a tantalum-rich organic phase and a raffinate, and performing a second stripping on the tantalum-rich organic phase to obtain a tantalum-rich solution; S6. Precipitating tantalum from the tantalum-rich liquid, and roasting the resulting precipitate after solid-liquid separation to obtain tantalum pentoxide; Precipitating niobium from the raffinate, and roasting the resulting precipitate after solid-liquid separation to obtain niobium pentoxide.

2. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that In step S1, the method for preparing low-grade niobium slag comprises the following steps: The titanium dioxide waste acid is subjected to a third extraction, and the obtained extract is washed and stripped with sodium hydroxide to obtain a niobium-containing alkali cake; the niobium-containing alkali cake is subjected to an acid-based dissolution and impurity removal to obtain the low-grade niobium slag.

3. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 2, It is characterized in that The extractant of the third extraction includes at least one of P204, P507, and P350; And / or, the pH value for optimal solubility and impurity removal is 0.5-3.

4. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that In step S2, at least one of the following features is included: (1) When dissolving the low-grade niobium slag, the mass volume ratio of solid to liquid is 1:1-1:5, and the unit is g / mL; (2) The concentration of the sulfuric acid is 1-6 mol / L; (3) The mass concentration of HF is 40%-50%; (4) The volume ratio of the sulfuric acid to the HF is 2-4:

1.

5. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that In step S3, at least one of the following features is included: (1) The main extractant includes at least one of TBP, MIBK, cyclohexanone and 2-octanol; (2) The volume percentage of the main extractant to the extractant is 20%-50%; (3) The volume percentage of the co-extraction agent to the extraction agent is 3%-8%; (4) The extraction phase ratio O / A of the first extraction is 1:1-3.

6. The method for extracting niobium and tantalum from waste titanium dioxide acid according to claim 1, It is characterized in that In step S4, the washing includes washing with sulfuric acid; and / or the impurity removal is performed by adjusting the pH to 3-5 by adding alkali.

7. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that In step S5, the extractant of the second extraction includes MIBK and 2-octanol; And / or, the second extraction is a multi-stage countercurrent extraction, and the extraction phase O / A ratio is 1:8-12.

8. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that The stripping agent of the first stripping and / or the second stripping is pure water.

9. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 1, It is characterized in that In step S6, the precipitating agent for tantalum precipitation and / or niobium precipitation is boric acid.

10. The method for extracting niobium and tantalum from titanium dioxide waste acid according to claim 9, It is characterized in that The following steps are also included: Add potassium salt to the filtrate after the tantalum and / or niobium precipitation, and evaporate and concentrate to obtain potassium fluoroborate.

Citation Information

Cited By

  • Method for preparing high-purity tantalum pentoxide and niobium pentoxide from niobium-tantalum iron ore

    CN120553756A

  • A method for preparing nano-sized tantalum powder by recycling waste tantalum resources

    CN123060107A