Polyimide aerogel fiber with gradient cross-linked structure and preparation method thereof

Through the preparation method of polyimide aerogel fibers with a gradient cross-linked structure, photosensitive group spinning solutions with different graft densities are used to form a three-dimensional interconnected nanofiber network, which solves the problem of polyimide aerogel fibers having high Strength and high toughness issues have improved the mechanical properties of the fiber and the weaving performance.

CN118854491AActive Publication Date: 2024-10-29JIANGNAN UNIV

Patent Information

Application Number
CN202411074648.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-29
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

It is difficult for existing polyimide airgel fibers to have both high strength and high toughness.

Method used

The polyimide airgel fiber with gradient cross-linked structure is prepared by extruding the spinning solution of photosensitive groups with different graft densities through a three-layer coaxial needle and irradiating it with an ultraviolet light source to form the cortex, middle layer and The three-dimensional interconnected nanofiber network of the core layer controls the grafting density of photosensitive groups to achieve a balance of mechanical strength and toughness.

Benefits of technology

It achieves high mechanical strength and high toughness of polyimide airgel fiber, improves the weaving performance of the fiber, and solves the problem of incompatible high strength and high toughness through microstructure control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854491A_ABST
    Figure CN118854491A_ABST
Patent Text Reader

Abstract

The invention relates to the field of aerogel preparation, in particular to a polyimide aerogel fiber with a gradient cross-linked structure and a preparation method of the polyimide aerogel fiber. The method comprises the following steps: copolymerizing diamine containing carboxyl or hydroxyl groups, other diamine and dicarboxylic anhydride, and controlling the grafting density of photosensitive groups to obtain photosensitive polyimide with different photosensitive group contents as a spinning solution; the polyimide aerogel fiber with the gradient cross-linked structure is obtained through three-layer coaxial wet spinning, ultraviolet irradiation, solvent replacement and normal-pressure drying, the polyimide aerogel fiber comprises a skin layer, a middle layer and a core layer, the skin layer is the most compact in structure, the core layer and the middle layer are of a porous structure of a three-dimensional interconnected nanofiber network, and the thickness of the core layer is larger than that of the middle layer. The filling power of the core layer structure is the highest; the photosensitive group grafting density of the photosensitive polyimide precursor solution of the spinning solution from the inner layer to the outer layer is gradually increased. By regulating and controlling the microstructure of the fiber, the problem that the aerogel fiber cannot have both high strength and high toughness is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerogel preparation, and in particular to a polyimide aerogel fiber with a gradient cross-linking structure and a preparation method thereof. Background Art

[0002] Aerogel is a new type of material with a three-dimensional porous structure using air as a dispersion medium. Due to its extremely low density, high porosity and low thermal conductivity, it has broad application prospects in aerospace, energy-saving buildings, clothing and other thermal insulation fields. Among them, aerogel fiber is an aerogel material with a one-dimensional macroscopic fiber structure. It combines the three-dimensional porous structure of aerogel and the flexibility of fiber, and has high porosity, low density, and low thermal conductivity (23-50mW m -1 K -1 ) as well as advantages such as weavability and wearability, it has the potential to become a new fiber material for efficient thermal management clothing.

[0003] Polyimide aerogel fiber prepared from polyimide, which is known as the "top material of the polymer material pyramid", plays an irreplaceable role in thermal protection textiles used in ultra-low and high temperature environments, such as space suits and fire suits, because of its excellent temperature resistance and excellent mechanical properties as well as the ultra-low thermal conductivity given by the three-dimensional porous structure of aerogel.

[0004] The porous structure and high porosity of aerogel fibers can give them excellent thermal insulation properties, but will inevitably lead to a decrease in the mechanical properties of aerogel fibers.

[0005] The mechanical strength of polyimide aerogel fibers reported so far is no higher than 15 MPa, and the fracture strain is no higher than 30%. [1] et al. prepared polyimide aerogel fibers through confined sol-gel strategy, with a mechanical strength of 11 MPa and a breaking strain of 25%. [2] et al. prepared polyimide aerogel fibers by freeze spinning strategy, and their mechanical strength was 10.6MPa, which was far different from that of solid fiber materials, and the fracture strain was 28.9%. It can be seen that although porous polyimide aerogel fibers have great application potential, it is a challenge to prepare polyimide aerogel fibers with both high strength and high toughness due to their high porosity and fragile mechanical properties. Therefore, the preparation of high-strength and high-toughness polyimide aerogel fibers is of great significance to the development of the aerogel fiber field.

[0006] [1]Xin Li, Guoqing Dong, Zengwei Liu, and Xuetong Zhang.PolyimideAerogel Fibers with Superior Flame Resistance,Strength,Hydrophobicity,andFlexibility Made via a Universal Sol-Gel Confined Transition Strategy.[J].ACSNano 2021 15(3),4759-4768.

[0007] [2] Yujie Wang, Ying Cui, Ziyu Shao, Weiwei Gao, Wei Fan, Tianxi Liu, HaoBai. Multifunctional polyimide aerogel textile inspired by polar bear hair forthermoregulation in extreme environments. [J]. Chemical Engineering Journal, 2020, 124623, 1385-8947. Summary of the invention

[0008] [Technical issues]

[0009] Existing polyimide aerogel fibers have difficulty in achieving both high strength and high toughness.

[0010] [Technical solution]

[0011] On the one hand, a method for preparing a polyimide aerogel fiber having a gradient cross-linking structure is provided, which comprises the following steps:

[0012] (1) subjecting a diamine containing a carboxyl group or a hydroxyl group, other diamines and a dibasic acid anhydride to a condensation reaction to form a polyamic acid; and subjecting the polyamic acid to chemical imidization to obtain a polyimide;

[0013] (2) using the polyimide obtained in step (1) as a raw material, preparing photosensitive polyimides with different grafting densities of photosensitive groups, and adding a photoinitiator and a polar aprotic solvent to respectively prepare photosensitive polyimide precursor solutions with different grafting densities of photosensitive groups;

[0014] (3) The photosensitive polyimide precursor solutions with different grafting densities of photosensitive groups prepared in step (2) are respectively used as spinning solutions and are defoamed, and then extruded from a three-layer coaxial needle, wherein the photosensitive group grafting densities of the photosensitive polyimide precursor solutions corresponding to the spinning solutions from the inner layer to the outer layer increase in sequence; wet gel fibers are formed by irradiation with ultraviolet light, and polyimide aerogel fibers with a gradient cross-linking structure are obtained by drawing, solvent replacement, drying at normal pressure, and collection; the polyimide aerogel fibers with a gradient cross-linking structure include a cortex layer, a middle layer, and a core layer, wherein the cortex layer structure is the densest, the core layer and the middle layer are porous structures of a three-dimensional interconnected nanofiber network, the core layer structure has the highest fluffiness, and the middle layer has the second-highest fluffiness.

[0015] In some embodiments, in step (1):

[0016] The diamine containing a carboxyl group or a hydroxyl group includes at least one of 3,5-diaminobenzoic acid (DABA) or 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP);

[0017] The other diamines include at least one of 4,4-diaminodiphenyl ether (ODA), 4,4'-diamino-2,2'-bistrifluoromethylbiphenyl (TFMB) or 2-(4-aminophenyl)-5-aminobenzimidazole (BIA);

[0018] The dibasic acid anhydride includes at least one of 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) or 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (A-ODPA).

[0019] In some embodiments, step (1) specifically includes the following steps:

[0020] Under the protection of inert gas, diamines containing carboxyl or hydroxyl groups and other diamines are completely dissolved in a polar aprotic solvent, and dibasic acid anhydride is added to carry out polycondensation reaction to obtain polyamic acid; high-temperature imidization is carried out to obtain polyimide containing carboxyl or hydroxyl groups in the molecular chain; wherein:

[0021] The molar ratio of the diamine containing carboxyl or hydroxyl groups to other diamines is 4:6 to 6:4; the ratio of the total molar number of the diamine containing carboxyl or hydroxyl groups and other diamines to the molar number of the dibasic acid anhydride is 1:(0.94 to 1.04); the ratio of the total mass of the diamine containing carboxyl or hydroxyl groups, other diamines and dibasic acid anhydride to the total mass of the diamine containing carboxyl or hydroxyl groups, other diamines, dibasic acid anhydride and polar aprotic solvent is (10 to 20):100.

[0022] In some embodiments, the temperature of the polycondensation reaction in step (1) is 0 to 25° C., and the time of the polycondensation reaction is 5 to 24 hours.

[0023] In some embodiments, the high temperature imidization reaction conditions in step (1) are: firstly heating to 120°C for reaction for 0.5-1h, then heating to 160°C for reaction for 0.5-1h, and finally heating to 200°C for reaction for 6-12h.

[0024] In some embodiments, in step (2):

[0025] The photosensitive group is acrylate.

[0026] In some embodiments, in step (2):

[0027] The photosensitive group includes at least one of hydroxyethyl methacrylate (HEMA), glycidyl methacrylate (GMA), or 2-hydroxyethyl acrylate (HEA).

[0028] In some embodiments, the method for preparing polyimide with different grafting densities of photosensitive groups in step (2) comprises the following steps:

[0029] Adding a photosensitive group-containing acrylate monomer, a dehydrating agent and a catalyst to a polar aprotic solvent and stirring until the solid is completely dissolved; then adding the mixture to the result of step (1), stirring at room temperature for 24 hours, separating the solution from the product, precipitating in water, and drying to obtain a photosensitive polyimide; wherein:

[0030] The acrylate monomer containing a photosensitive group includes at least one of hydroxyethyl methacrylate, glycidyl methacrylate or 2-hydroxyethyl acrylate;

[0031] Dehydrating agents include N,N'-dicyclohexylcarbodiimide or 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride;

[0032] The catalyst is 4-dimethylaminopyridine;

[0033] The molar ratio of the acrylate monomer containing a photosensitive group to the diamine containing a carboxyl group or a hydroxyl group is (0.1-100):100;

[0034] The molar ratio of the acrylate monomer containing a photosensitive group: the dehydrating agent: the catalyst is 10:10:1.

[0035] In some embodiments, the photoinitiator in step (2) includes at least one of Irgacure-184, Irgacure-2959, Irgacure-651, Irgacure-369, Irgacure-907, Irgacure-1300, Irgacure-784, Irgacure-250, Irgacure-819, Irgacure819DW, Darocur-4265, Darocur BP, Darocur MBF, DarocurTPO or Darocur-1173, and the amount of the photoinitiator is 0.5-2wt% of the total mass of the photosensitive polyimide precursor solution, and the solid content of the photosensitive polyimide precursor solution is 5-30wt%.

[0036] In some embodiments, in the method for preparing polyimide with different grafting densities of photosensitive groups in step (1) or step (2), the polar aprotic solvent is N-methylpyrrolidone.

[0037] In some embodiments, the polar aprotic solvent used in preparing the photosensitive polyimide precursor solution in step (2) includes N-methylpyrrolidone, N,N-dimethylacetamide or N,N-dimethylformamide.

[0038] In some embodiments, in step (3):

[0039] The photosensitive group grafting density of the photosensitive polyimide precursor solution corresponding to the spinning solution from the inner layer to the outer layer is 20%, 50% and 100% respectively.

[0040] In some embodiments, in step (3), the extrusion speed of the syringe pump used for three-layer coaxial needle extrusion is 10 to 100 μL min -1 The dimensions of the three-layer coaxial needle are: the core layer diameter is 100-300 μm; the middle layer diameter is 400-700 μm; the skin layer diameter is 1.07-1.35 mm; the power of the ultraviolet light source is 0.3-3 W cm -2 The UV light source irradiation time is 0.01 to 3 minutes; the drafting multiple is 1 to 6 times, and the collection speed is 0.3 to 15 minutes. -1 .

[0041] In some embodiments, the solvent used for solvent replacement in step (3) includes at least one of water, acetone, ethanol, methanol, isopropanol or n-hexane, the temperature of solvent replacement is 25-100° C., the time of solvent replacement is 24-96 h, and the number of replacements is 3-5 times.

[0042] In some embodiments, the temperature of normal pressure drying in step (3) is 25 to 100° C., and the time is 2 to 48 hours.

[0043] On the other hand, a polyimide aerogel fiber with a gradient cross-linking structure prepared by the aforementioned method is provided.

[0044] In another aspect, the invention provides application of the aforementioned polyimide aerogel fiber with gradient cross-linking structure in the field of intelligent thermal management.

[0045] In some embodiments, the polyimide aerogel fiber with a gradient cross-linking structure is used in the fields of architectural decoration, aerospace, or firefighting clothing.

[0046] [Beneficial Effects]

[0047] (1) Different from the existing coaxial polyimide aerogel fiber, which has no interaction between the skin and core layers and poor mechanical properties, the present invention provides a polyimide aerogel fiber with a gradient cross-linking structure and a preparation method thereof, wherein polyimide with different photosensitive group grafting densities is used as a spinning solution, wherein the photosensitive group grafting densities of the photosensitive polyimide corresponding to the spinning solutions from the inner layer to the outer layer increase in sequence, and the gel fiber is obtained by UV-assisted coaxial wet spinning based on a three-layer coaxial needle, which is subjected to solvent replacement in a coagulation bath and dried at normal pressure to obtain a polyimide aerogel fiber with a gradient cross-linking structure, and the three-layer gradient cross-linking structure polyimide aerogel fiber is successfully formed in one piece, wherein the three-layer gradient cross-linking structure includes a skin layer, an intermediate layer and a core layer, wherein the skin layer structure is the densest, the core layer and the intermediate layer are porous structures of a three-dimensional interconnected nanofiber network, the core layer structure has the highest fluffiness, and the intermediate layer has the highest fluffiness. Based on the above-mentioned specific structure, the polyimide aerogel fiber is endowed with high mechanical strength, high toughness and excellent thermal insulation performance;

[0048] (2) The polyimide aerogel fiber of the present invention has a three-layer gradient cross-linked structure. Under ultraviolet light irradiation, the photosensitive groups in different layers of spinning solution quickly undergo free radical polymerization reaction to achieve the integrated molding of the gradient cross-linked structure aerogel fiber; wherein, as the cross-linking density increases, the mechanical strength increases, so the high cross-linking degree of the skin layer provides the mechanical strength of the fiber, and the low cross-linking degree of the core layer provides the flexibility and toughness of the fiber; that is, the skin layer adopts a high photosensitive group grafting density to provide high mechanical strength for the fiber, and the core layer adopts a low photosensitive group grafting density to provide toughness and flexibility for the fiber. At the same time, due to the compatibility of the spinning solution, the different layers are chemically cross-linked by the photosensitive groups during the preparation process, which further improves the mechanical properties of the fiber. Therefore, the triaxial gradient cross-linked polyimide aerogel fiber of the present invention achieves a balance between strength and toughness, and gives the fiber better weaving properties; further, the use of fluorine-containing dibasic acid anhydride or diamine can effectively reduce the surface tension and reduce the shrinkage rate of the aerogel fiber during normal pressure drying. The method of the present invention solves the problem that aerogel fibers cannot have both high strength and high toughness by regulating the fiber microstructure;

[0049] (3) The method of the present invention first polymerizes a diamine containing a carboxyl structure or a hydroxyl structure with a dibasic acid anhydride compound to form polyamic acid, and obtains polyimide through chemical imidization; the grafting density is controlled by controlling the content of the photosensitive compound to obtain a fluorinated polyimide spinning solution with different photosensitive group contents. The defoamed spinning solution is then extruded through a three-axis needle, and under ultraviolet light irradiation, the photosensitive groups rapidly undergo free radical polymerization to form gel networks of different strengths to obtain stable gel fibers. At the same time, due to the compatibility of different layers of spinning solution, chemical crosslinking exists between different layers. After obtaining the gel fiber, it enters a coagulation bath for solvent replacement, and is dried at normal pressure to obtain a polyimide aerogel fiber with a gradient crosslinking structure;

[0050] (4) The polyimide aerogel fiber with a gradient cross-linking structure based on coaxial spinning and normal pressure drying of the present invention has a gradient cross-linking structure because the grafting density of the photosensitive groups of the inner and outer spinning solutions is different. In addition, the photosensitive group acrylate is introduced into the polyimide through polycondensation and Steglich esterification reaction. The coaxial wet spinning process directly applies an ultraviolet light source to form a polyimide wet gel fiber, and then the polyimide aerogel fiber with a gradient cross-linking structure is prepared through solvent replacement and normal pressure drying.

[0051] (5) The present invention synthesizes organic soluble photosensitive polyimide, extrude it through a three-axis needle, irradiate it with ultraviolet light, and then perform ultraviolet crosslinking, solvent replacement, and normal pressure drying on the spinning solution to form a polyimide aerogel fiber with a gradient crosslinking structure. The SEM image proves the formation of the gradient crosslinking structure, and the stress-strain curve also proves that the obtained fiber has a strength and elongation at break that exceed the average level of current aerogel fibers, and simultaneously achieves a balance between the strength and toughness of the polyimide aerogel fiber, which is greatly improved compared to the existing polyimide aerogel fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is a scanning electron microscope image of the polyimide aerogel fiber with a gradient cross-linking structure prepared in Example 1;

[0053] Figure 2 The test results of nuclear magnetic resonance hydrogen spectrum of the photosensitive polyimide and polyimide with different grafting densities in Example 1;

[0054] Figure 3 Optical photograph showing the flexibility and continuity of the polyimide aerogel fiber with a gradient cross-linking structure prepared in Example 1;

[0055] Figure 4 This is an optical display photograph showing that the polyimide aerogel fiber with a gradient cross-linking structure prepared in Example 1 can bear a weight of 200 g;

[0056] Figure 5 These are the stress-strain curves of the polyimide aerogel fiber with a gradient cross-linking structure (GCPAF-1) prepared in Example 1 and the polyimide aerogel fibers with a single component and different grafting densities (CPI-20, CPI-50, and CPI-100). DETAILED DESCRIPTION

[0057] Test method:

[0058] An electronic universal testing machine (Model E42, MTS, USA) was used with a sensor of 50N and 0.8mm s -1 , the mechanical properties of aerogel fibers were tested in tensile mode.

[0059] The microstructure of the aerogel fibers was observed using a field emission scanning electron microscope (SU8600, Japan).

[0060] Example 1

[0061] A method for preparing a polyimide aerogel fiber with a gradient cross-linking structure comprises the following steps:

[0062] (1) Preparation of copolymerized polyimide:

[0063] In a three-necked round-bottom flask, under nitrogen protection, 3,5-diaminobenzoic acid (DABA, 0.7608 g), 4,4-diaminodiphenyl ether (ODA, 1.001 g) and N-methylpyrrolidone (NMP, 25 mL) were added in sequence, and stirred until DABA and ODA were completely dissolved; then 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA, 4.4423 g) was added, and the mixture was reacted at 25°C for 24 h; the temperature was raised to 120°C and kept for reaction for 1 h, and then the temperature was raised to 160°C and kept for reaction for 1 h, and then the temperature was raised to 200°C and kept for reaction for 10 h to obtain a soluble polyimide (copolyimide) solution;

[0064] (2) Preparation of photosensitive polyimides with different grafting densities grafted with hydroxyethyl methacrylate:

[0065] Preparation of photosensitive polyimide with 100% hydroxyethyl methacrylate grafting amount: hydroxyethyl methacrylate (HEMA, 5 mmol), N,N'-dicyclohexylcarbocyanine (5 mmol) and 4-dimethylaminopyridine (0.50 mmol) were added to N-methylpyrrolidone (NMP, 6 mL) in sequence and stirred until the solid disappeared, and then added to the soluble polyimide solution of step (1), and stirred at room temperature for 24 hours to cause Steglich esterification reaction until a precipitate was generated; the upper layer solution was obtained by centrifugation from the product, and then the solution was precipitated into deionized water, repeatedly washed, and dried to obtain a photosensitive polyimide with 100% grafting amount;

[0066] Preparation of photosensitive polyimide with 50% hydroxyethyl methacrylate grafting amount: Referring to the preparation steps of photosensitive polyimide with 100% hydroxyethyl methacrylate grafting amount, the only difference is that the amount of reactants is changed, hydroxyethyl methacrylate (HEMA, 2.5mmol), N,N'-dicyclohexylcarbocyanine (2.5mmol) and 4-dimethylaminopyridine (0.25mmol), and finally a photosensitive polyimide with 50% grafting amount is obtained;

[0067] Preparation of photosensitive polyimide with 20% hydroxyethyl methacrylate grafting amount: Referring to the preparation steps of photosensitive polyimide with 100% hydroxyethyl methacrylate grafting amount, the only difference is that the amount of reactants is changed, hydroxyethyl methacrylate (HEMA, 1mmol), N,N'-dicyclohexylcarbocyanine (1mmol) and 4-dimethylaminopyridine (0.1mmol), and finally a photosensitive polyimide with 20% grafting amount is obtained;

[0068] Note: The above grafting amount of hydroxyethyl methacrylate is based on 100% grafting amount of hydroxyethyl methacrylate, which means that the molar ratio of grafted hydroxyethyl methacrylate to the carboxyl content in the copolymerized polyimide prepared in the previous step is 1:1, which is the theoretical grafting amount. The gradient design here is carried out according to the theoretical grafting amount.

[0069] (3) Preparation of photosensitive polyimide precursor solution:

[0070] According to the mass ratio of photosensitive polyimide: N-methylpyrrolidone: photoinitiator being 15:83:2, the photosensitive polyimides with different grafting amounts obtained above were respectively dissolved in N-methylpyrrolidone, and then the photoinitiator Irgacure-819 was added and stirred for 20 minutes to obtain photosensitive polyimide precursor solutions with different grafting amounts; the solid content of the photosensitive polyimide precursor solution was 15wt%;

[0071] (4) Preparation of polyimide aerogel fibers:

[0072] The photosensitive polyimide precursor solutions with different grafting amounts prepared in step (3) were used as spinning solutions and, after degassing, were extruded from a three-layer coaxial needle via an injection pump, wherein the hydroxyethyl methacrylate grafting amounts of the photosensitive polyimide corresponding to the spinning solutions from the inner layer to the outer layer were 20%, 50% and 100% respectively; the coaxial needle dimensions were: the core layer diameter was 190 μm, the middle layer diameter was 400 μm, and the skin layer diameter was 1.07 mm; the extrusion speed of the injection pump was 50 μL min -1 ; 0.6W cm -2 After 15 seconds of ultraviolet light irradiation, wet gel fibers were formed. After drawing, solvent replacement, normal pressure drying and collection, gradient cross-linked polyimide aerogel fibers were obtained, which were recorded as GCPAF-1. The drawing multiple was 2 times and the collection speed was 0.6 m / min. -1 The solvent used for solvent replacement was ethanol, the temperature was 25°C, the time was 48h, and the number of replacements was 4 times; the temperature for normal pressure drying was 25°C, and the time was 24h.

[0073] Figure 1 is a scanning electron microscope image of the polyimide aerogel fiber with a gradient cross-linking structure prepared in Example 1; Figure 1 It can be seen that the obtained polyimide aerogel fiber successfully formed a gradient cross-linked structure, including a cortex, a middle layer and a core layer, among which the cortex structure is the densest, the core layer and the middle layer are porous structures of three-dimensional interconnected nanofiber networks, the core layer structure has the highest fluffiness, and the middle layer is second to third.

[0074] Figure 2The test results of nuclear magnetic resonance hydrogen spectrum of the photosensitive polyimide and polyimide with different grafting densities in Example 1 are shown in the figure. It can be seen from the figure that the peaks at 5.8ppm, 4.6ppm and 4.3ppm correspond to the hydrogen on the unsaturated double bond and the hydrogen on the methylene of the fatty chain on the photosensitive polyimide (PPI), respectively, corresponding to H1, H2 and H3 marked on the structural formula. At the same time, the intensity of the characteristic peak increases with the increase of the grafting amount. The above analysis proves that HEMA is successfully grafted on the side chain of polyimide (PI) through Stiglitz esterification reaction, thereby confirming the successful synthesis of photosensitive polyimide (PPI).

[0075] Figure 3 The optical photographs show the flexibility and continuity of the polyimide aerogel fiber with gradient cross-linking structure prepared in Example 1; Figure 3 It can be seen that polyimide aerogel fibers with a gradient cross-linking structure of a certain length can be entangled without breaking, which confirms that GCPAF-1 has good flexibility and continuity.

[0076] Figure 4 This is an optical display photograph showing that the polyimide aerogel fiber with a gradient cross-linking structure prepared in Example 1 can withstand a weight of 200 g; Figure 4 It can be seen that the polyimide aerogel fiber with a gradient cross-linking structure in Example 1 can withstand a 200 g weight without breaking, thereby confirming that the fiber has good mechanical properties.

[0077] Comparative Example 1

[0078] A method for preparing a polyimide aerogel fiber with a gradient cross-linked structure, referring to Example 1, except that: in step (4), the amounts of hydroxyethyl methacrylate grafted with the photosensitive polyimide corresponding to the spinning solutions from the inner layer to the outer layer are 100%, 50% and 20% respectively, and the obtained gradient cross-linked polyimide aerogel fiber is recorded as GCPAF-2.

[0079] The experimental results show that the grafting amount of hydroxyethyl methacrylate from the inside to the outside is a gradient of 100%, 50% and 20% respectively. Due to the 20% photosensitive group grafting density in the outermost layer, the sol-gel transition of the fiber takes longer time, and it is difficult to match the overall spinning speed during the spinning process, and a continuous three-layer coaxial structure cannot be obtained. Therefore, the aerogel fiber with a gradient cross-linked structure cannot be formed.

[0080] Comparative Example 2

[0081] A method for preparing polyimide aerogel fiber, referring to Example 1, except that only 20% of photosensitive polyimide grafted with hydroxyethyl methacrylate is used as the spinning solution, and ultraviolet-assisted wet spinning is performed by extrusion through a needle with an inner diameter of 1.07 mm. The obtained cross-linked polyimide aerogel fiber is recorded as CPI-20.

[0082] Comparative Example 3

[0083] A method for preparing polyimide aerogel fiber, referring to Example 1, except that only 50% of photosensitive polyimide grafted with hydroxyethyl methacrylate is used as the spinning solution, and ultraviolet-assisted wet spinning is performed by extrusion through a needle with an inner diameter of 1.07 mm. The obtained cross-linked polyimide aerogel fiber is recorded as CPI-50.

[0084] Comparative Example 4

[0085] A method for preparing polyimide aerogel fiber, referring to Example 1, except that only 100% of photosensitive polyimide grafted with hydroxyethyl methacrylate is used as the spinning solution, and ultraviolet-assisted wet spinning is performed by extrusion with a needle with an inner diameter of 1.07 mm. The obtained cross-linked polyimide aerogel fiber is recorded as CPI-100.

[0086] Figure 5 The stress-strain curves of the polyimide aerogel fiber with gradient cross-linking structure (GCPAF-1) and the polyimide aerogel fibers with different grafting densities (CPI-20, CPI-50, CPI-100) prepared in Example 1 are shown in FIG. Figure 5 It can be seen that the polyimide aerogel fiber with a gradient cross-linking structure has a higher breaking strength of 24.5 MPa and a higher breaking strain of 49.1% than the cross-linked polyimide aerogel fiber with a single structure. This confirms that the aerogel fiber obtained by designing a three-layer coaxial structure of the aerogel fiber and UV-assisted coaxial wet spinning has a strength that is better than the current aerogel fiber level of 8 to 15 MPa, and the toughness is significantly improved, thereby realizing the preparation of high-strength and high-toughness aerogel fibers.

[0087] Comparative Example 5

[0088] The mechanical properties of polyimide aerogel fibers prepared in the current literature were investigated. [1] et al. prepared polyimide aerogel fibers through confined sol-gel strategy, with a mechanical strength of 11 MPa and a breaking strain of 25%. [2]et al. prepared polyimide aerogel fibers using freeze spinning strategy, with a mechanical strength of 10.6 MPa and a fracture strain of 28.9%. It can be seen that it is a challenge to prepare polyimide aerogel fibers with both high strength and high toughness.

[0089] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing a polyimide aerogel fiber with a gradient cross-linking structure, characterized in that: The steps include: (1) subjecting a diamine containing a carboxyl group or a hydroxyl group, other diamines and a dibasic acid anhydride to a condensation reaction to form a polyamic acid; and subjecting the polyamic acid to chemical imidization to obtain a polyimide; (2) using the polyimide obtained in step (1) as a raw material, preparing photosensitive polyimides with different grafting densities of photosensitive groups, and adding a photoinitiator and a polar aprotic solvent to respectively prepare photosensitive polyimide precursor solutions with different grafting densities of photosensitive groups; (3) The photosensitive polyimide precursor solutions with different grafting densities of photosensitive groups prepared in step (2) are respectively used as spinning solutions and are defoamed, and then extruded from a three-layer coaxial needle, wherein the photosensitive group grafting densities of the photosensitive polyimide precursor solutions corresponding to the spinning solutions from the inner layer to the outer layer increase in sequence; wet gel fibers are formed by irradiation with ultraviolet light, and polyimide aerogel fibers with a gradient cross-linking structure are obtained by drawing, solvent replacement, drying at normal pressure, and collection; the polyimide aerogel fibers with a gradient cross-linking structure include a cortex layer, a middle layer, and a core layer, wherein the cortex layer structure is the densest, the core layer and the middle layer are porous structures of a three-dimensional interconnected nanofiber network, the core layer structure has the highest fluffiness, and the middle layer has the second-highest fluffiness.

2. The method according to claim 1, characterized in that In step (1): The diamine containing a carboxyl group or a hydroxyl group includes at least one of 3,5-diaminobenzoic acid or 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane; The other diamines include at least one of 4,4-diaminodiphenyl ether, 4,4'-diamino-2,2'-bistrifluoromethylbiphenyl or 2-(4-aminophenyl)-5-aminobenzimidazole; The dibasic acid anhydride includes at least one of 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic anhydride) or 2,3,3',4'-diphenyl ether tetracarboxylic anhydride.

3. The method according to claim 1, characterized in that In step (2): The photosensitive group is acrylate.

4. The method according to claim 1, characterized in that: In step (3): The photosensitive group grafting density of the photosensitive polyimide precursor solution corresponding to the spinning solution from the inner layer to the outer layer is 20%, 50% and 100% respectively.

5. The method according to claim 1, characterized in that Step (1) specifically includes the following steps: Under the protection of inert gas, diamines containing carboxyl or hydroxyl groups and other diamines are completely dissolved in a polar aprotic solvent, and dibasic acid anhydride is added to carry out polycondensation reaction to obtain polyamic acid; high-temperature imidization is carried out to obtain polyimide containing carboxyl or hydroxyl groups in the molecular chain; wherein: The molar ratio of the diamine containing carboxyl or hydroxyl groups to other diamines is 4:6 to 6:4; the ratio of the total molar number of the diamine containing carboxyl or hydroxyl groups and other diamines to the molar number of the dibasic acid anhydride is 1:(0.94 to 1.04); the ratio of the total mass of the diamine containing carboxyl or hydroxyl groups, other diamines and dibasic acid anhydride to the total mass of the diamine containing carboxyl or hydroxyl groups, other diamines, dibasic acid anhydride and polar aprotic solvent is (10 to 20):

100.

6. The method according to claim 1, characterized in that The method for preparing polyimide with different grafting density of photosensitive groups in step (2) comprises the following steps: Adding a photosensitive group-containing acrylate monomer, a dehydrating agent and a catalyst to a polar aprotic solvent and stirring until the solid is completely dissolved; then adding the mixture to the resultant of step (1), stirring at room temperature for reaction, separating the solution from the product, precipitating in water, and drying to obtain a photosensitive polyimide; wherein: The acrylate monomer containing a photosensitive group includes at least one of hydroxyethyl methacrylate, glycidyl methacrylate or 2-hydroxyethyl acrylate; Dehydrating agents include N,N'-dicyclohexylcarbodiimide or 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; The catalyst is 4-dimethylaminopyridine; The molar ratio of the acrylate monomer containing a photosensitive group to the diamine containing a carboxyl group or a hydroxyl group is (0.1-100):100; The molar ratio of the acrylate monomer containing a photosensitive group: the dehydrating agent: the catalyst is 10:10:

1.

7. The method according to claim 1, characterized in that The photoinitiator in step (2) includes at least one of Irgacure-184, Irgacure-2959, Irgacure-651, Irgacure-369, Irgacure-907, Irgacure-1300, Irgacure-784, Irgacure-250, Irgacure-819, Irgacure819DW, Darocur-4265, Darocur BP, Darocur MBF, Darocur TPO or Darocur-1173, and the amount of the photoinitiator is 0.5-2wt% of the total mass of the photosensitive polyimide precursor solution, and the solid content of the photosensitive polyimide precursor solution is 5-30wt%.

8. The method according to claim 1, characterized in that In step (3), the extrusion speed of the syringe pump used for the three-layer coaxial needle extrusion is 10-100 μL min -1 The dimensions of the three-layer coaxial needle are: the core layer diameter is 100-300 μm; the middle layer diameter is 400-700 μm; the skin layer diameter is 1.07-1.35 mm; the power of the ultraviolet light source is 0.3-3 W cm -2 The UV light source irradiation time is 0.01 to 3 minutes; the drafting multiple is 1 to 6 times, and the collection speed is 0.3 to 15 minutes. -1 .

9. The polyimide aerogel fiber having a gradient cross-linking structure obtained by the method according to any one of claims 1 to 8.

10. Application of the polyimide aerogel fiber with a gradient cross-linking structure as claimed in claim 9 in the field of intelligent thermal management.

Citation Information

Patent Citations

  • Polyimide aerogel fiber as well as preparation method and application thereof

    CN113355772A

  • Aerogel phase change intelligent fiber with adjustable bending rigidity as well as preparation method and application thereof

    CN113550143A

  • Normal-pressure drying preparation method and application of polyimide aerogel product

    CN113818098A

  • Coaxial spinning-based polyimide aerogel fiber and preparation method thereof

    CN114908438A

  • Polyimide aerogels with reduced shrinkage from isothermal aging

    US10723857B1

Cited By

  • Aerogel fiber prepared from waste aramid fiber under extremely cold condition and method thereof

    CN120666459A

  • Preparation method of super-hydrophobic photocuring polyimide electrostatic spinning film

    CN120818946A