Method for controlling oxide scale defects on surface of thin-gauge AH36 steel

By controlling the slab composition and rolling process parameters of AH36 steel, including converter smelting, refining and multiple descaling treatments, the problem of iron oxide defects on the surface of AH36 steel is solved, and rolling without increasing production costs High-quality AH36 steel with a thickness of less than 8mm can be produced to meet the needs of the hull structure.

CN118904947APending Publication Date: 2024-11-08SHANDONG IRON & STEEL CO LTD

Patent Information

Application Number
CN202410972100.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has failed to effectively solve the problem of defects in the surface of AH36 steel, especially on the premise of ensuring rolling stability and not increasing the production cost of steel plates, it is difficult to achieve systematic control of the surface of thin-specification AH36 steel.

Method used

By controlling the specific parameters of each process flow by controlling the composition of the slab, slab heating, coarse scale descaling, fine rolling, secondary scale descaling, and winding, converter smelting → LF refining → RH refining → continuous casting → slab heating → coarse removal The process of scale → finish rolling → secondary scale descaling → coiling reduces Si content, uses the superposition of large flow and small flow descaling to perform coarse phosphorus removal, and uses odd + even pass phases during finishing rolling The combined secondary descaling method controls the cooling amount of the plate and the phosphorus removal water flow.

Benefits of technology

Without increasing the production cost of steel plates, the oxidation and scaling of AH36 steel is effectively suppressed, the surface quality of the intermediate billet is improved, and the formation of oxidized iron sheet defects during the rolling process is avoided, and the surface of thin AH36 steel with a thickness of <8mm is smooth and of good quality. Meet the use needs of steel for ship slabs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904947A_ABST
    Figure CN118904947A_ABST
Patent Text Reader

Abstract

The invention discloses a method for controlling surface oxide scale defects of thin-gauge AH36 steel, which comprises the following steps: accurately controlling specific parameters of each process flow of converter smelting, LF (ladle furnace) refining, RH (Ruhrstahl Heraeus) refining, continuous casting, slab heating, rough descaling, finish rolling, secondary descaling and coiling, and reducing the Si content in the converter smelting process according to the weight percentage of 0.12-0.15%. And before finish rolling, rough dephosphorization is carried out in the mode that large-flow descaling and small-flow descaling are overlapped, secondary descaling is carried out through cooperation of odd-number passes and even-number passes in the finish rolling process, and the thin-gauge AH36 steel is obtained. On the premise that the production cost of the steel plate is not increased and the rolling stability is guaranteed, the control problem of the oxide scale defect in the AH36 steel rolling process is solved, the obtained thin-gauge AH36 steel with the thickness smaller than 8 mm is smooth in surface and good in quality, the use requirement of ship plate steel for the thin-gauge AH36 steel is met, and the thin-gauge AH36 steel can be widely applied to main stress parts of a ship body structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel rolling, and in particular relates to a method for controlling iron oxide scale defects on the surface of thin-gauge AH36 steel. Background Art

[0002] AH36 steel is a high-strength steel plate for marine structures. It has good weldability, formability, toughness and corrosion resistance. It can meet the use requirements in complex environments and is widely used in ships, marine engineering, bridges and other fields. In shipbuilding, AH36 steel is used in the main stress-bearing parts of the hull structure, such as decks, bottoms, and sides. Its high strength, good toughness and corrosion resistance can ensure the stability and safety of the hull structure, improve the carrying capacity and service life of the ship, and play an important role in the development of the shipbuilding industry. Based on the complexity of the use environment of AH36 steel, good surface quality of the steel grade can significantly improve the oxidation resistance and corrosion resistance of the steel grade. Therefore, more stringent requirements are also put forward for the surface quality control process of AH36 steel.

[0003] The surface quality of steel plates has always been one of the key factors restricting the improvement of the overall quality of hot-rolled plates. Surface quality problems caused by the iron oxide scale on the surface of steel plates occur frequently. The grinding or modification of steel plates seriously affects the production efficiency and brand image. Controlling the iron oxide scale on steel plates is very necessary to improve the surface quality of hot-rolled steel plates. At present, the iron oxide scale defects on the surface of hot-rolled strip steel are mainly achieved by maintaining or optimizing the strip descaling equipment, adjusting the descaling timing and adjusting the process parameters. CN113877963A discloses a control method for the pressure-in of the iron oxide scale on the surface of hot-rolled silicon-controlled strip steel. Effective control measures are taken for the key points of the slab heating, rough rolling and finishing rolling processes, and the iron oxide scale of the silicon-controlled hot-rolled strip steel is controlled. CN117181817A discloses a method for controlling the iron scale defects of hot-rolled thin-gauge high-strength pickled plates. The slab is heated and then taken out of the furnace. The heated slab is descaled and rough-rolled in sequence to obtain an intermediate slab; the intermediate slab is descaled and finish-rolled in sequence; the strip after finish-rolling is laminar-cooled and coiled, which solves the problem of surface iron scale when rolling thin-gauge high-strength hot-rolled pickled plates. The invention is mainly aimed at controlling the iron scale defects of pickled plates.

[0004] As a typical hot-rolled strip steel, the peeling of the iron oxide scale on the surface of AH36 steel is very likely to cause corrosion, thus affecting the quality of the steel. Currently, relevant patents and literature have not yet given a systematic control method to effectively solve the iron oxide scale defect on the surface of AH36 steel while ensuring rolling stability. Summary of the invention

[0005] The present invention provides a method for controlling iron oxide scale defects on the surface of thin-gauge AH36 steel. The purpose of the present invention is to form a complete set of methods for controlling iron oxide scale defects on the surface of thin-gauge AH36 steel by controlling specific parameters of each process flow including slab composition, slab heating, rough descaling, fine rolling, secondary descaling and coiling, under the premise of ensuring rolling stability and not increasing the production cost of steel plates, so as to obtain thin-gauge AH36 steel with a thickness of less than 8 mm, effectively solve the problem of iron oxide scale on the surface of thin-gauge AH36 steel when rolling, and achieve the standard of smooth steel surface and good surface quality.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for controlling iron oxide scale defects on the surface of thin-gauge AH36 steel comprises: converter smelting→LF refining→RH refining→continuous casting→slab heating→rough descaling→finishing rolling→secondary descaling→coiling, wherein the Si content is reduced during the converter smelting process, the Si content is 0.12-0.15% by weight, rough dephosphorization is performed before finish rolling by superimposing large flow and small flow descaling, and secondary descaling is performed by combining odd and even passes during finish rolling.

[0008] The specific steps of the above preparation method are as follows:

[0009] (1) Slab composition control: Continuously cast slabs are obtained through “converter smelting → LF refining → RH refining → continuous casting”, in which the Si content is reduced during the converter smelting process;

[0010] (2) Slab heating: the continuous casting slab obtained in step (1) is placed in a heating furnace with an oxygen content of less than 3.5% for heating and then taken out of the furnace;

[0011] (3) Rough dephosphorization: The slab heated in step (2) is subjected to rough dephosphorization by superimposing large-flow and small-flow descaling processes to achieve the standard of completely removing the furnace-born iron oxide scale on the surface of the slab, thereby obtaining an intermediate slab;

[0012] (4) Finish rolling: The intermediate billet obtained in step (3) is subjected to finish rolling, with the number of rolling passes being 7 to 9;

[0013] (5) Secondary descaling: During finishing rolling, descaling between stands is turned on, and secondary dephosphorization is performed by combining odd and even passes;

[0014] (6) Coiling: The finished rolled slab obtained in step (5) is coiled to obtain thin-gauge AH36 steel with a thickness of less than 8 mm.

[0015] Furthermore, the chemical composition of the slab in step (1) is as follows by weight: C: 0.15-0.20%, Si: 0.12-0.15%, S: 0.001-0.004%, P: 0.010-0.020%, Mn: 1.10-1.50%, Al: 0.020-0.050%, Cr: ≤0.03%, Nb: 0.015-0.020%, V: ≤0.01%, Ti: 0.010-0.015%, Cu: ≤0.02%, Ni: ≤0.01%, and the remainder is iron and unavoidable impurity elements.

[0016] Furthermore, in step (2), the furnace temperature is controlled at 1230-1250° C., and the total furnace time is ≤190 min.

[0017] Furthermore, the method of superimposing the large flow rate and small flow rate descaling in step (3) means that during the dephosphorization process, the large flow rate and small flow rate descaling nozzles are opened simultaneously to dephosphorize the slab. The dephosphorization schematic diagram is shown in Figure 1 .

[0018] Furthermore, the high-flow descaling water pressure in step (3) is 19-23 MPa, and the flow rate is 430-460 m 3 / h; the small flow descaling water pressure is 22-24MPa, and the flow rate is 140-165m 3 / h.

[0019] Furthermore, in step (4), the start rolling temperature of the finishing rolling is controlled at 1080-1100°C, and the final rolling temperature is controlled at 820-840°C.

[0020] Furthermore, the odd-numbered + even-numbered passes in step (5) are 1, 2, 3, 5, 6, and 7 passes of rolling, 1, 2, 3, and 5 passes use a large flow rate for dephosphorization, and 6 and 7 passes use a small flow rate for descaling.

[0021] Furthermore, the coiling temperature in step (6) is 850-900°C.

[0022] Beneficial effects:

[0023] The present invention controls the composition of the slab and reduces the Si content of AH36 steel. The Si content of 0.12-0.15% can effectively inhibit the occurrence of oxidation scaling of AH36 steel and promote oxide peeling. Before finishing rolling, a large flow rate and a small flow rate descaling are superimposed to remove phosphorus, which can accurately control the cooling amount of the plate, inhibit the scaling of the AH36 steel oxide scale, and further improve the surface quality of the intermediate billet. In the secondary descaling process, an odd number + an even number of dephosphorization passes are combined to remove scale in 6 rolling passes, namely 1, 2, 3, 5, 6, and 7, to enhance the descaling effect, accurately control the dephosphorization water flow, and effectively avoid the generation of oxide scale defects during the rolling process. The present invention forms a complete set of methods for controlling iron oxide scale defects on the surface of thin-gauge AH36 steel without increasing the production cost of steel plates and ensuring rolling stability, thereby solving the problem of controlling iron oxide scale defects during the rolling process of AH36 steel. The obtained thin-gauge AH36 steel with a thickness of less than 8 mm has a smooth surface and good quality, meets the use requirements of thin-gauge AH36 steel for ship plates, and can be widely used in the main stress-bearing parts of the hull structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the phosphorus removal method with a large flow rate and a small flow rate superimposed;

[0025] Figure 2 This is the surface quality diagram of AH36 steel obtained in Example 1;

[0026] Figure 3 This is the surface quality diagram of AH36 steel obtained in Example 2;

[0027] Figure 4 This is the surface quality diagram of AH36 steel obtained in Example 3. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be specifically described below in conjunction with the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0029] Example 1

[0030] A thin gauge AH36 steel, whose chemical composition by weight percentage is: C: 0.15%, Si: 0.14%, S: 0.003%, P: 0.012%, Mn: 1.34%, Al: 0.025%, Cr: 0.03%, Nb: 0.016%, V: 0.01%, Ti: 0.014%, Cu: 0.01%, Ni: 0.01%, the balance is iron and unavoidable impurity elements, the process flow is: converter smelting → LF refining → RH refining → continuous casting → slab heating → rough descaling → finishing rolling → secondary descaling → coiling, the specific steps are as follows:

[0031] (1) Converter smelting: molten iron is added to a 100t converter for smelting, the final temperature is 1640°C, the final carbon content of the converter is 0.08%, and deoxidation and alloying are performed during the converter tapping process. The addition amounts of each component are as follows: silicon manganese alloy (FeMn68Si18): 9.8kg / t, high carbon ferromanganese (FeMn68C7.0): 11.56kg / t, ferroniobium (FeNb60-B): 0.26kg / t, ferrotitanium (FeTi30-A): 1.1kg / t, aluminum ferromanganese (FeMnAl55): 2.5kg / t, aluminum particles 0.5kg / t, aluminum wire Φ13: 1m / t;

[0032] (2) LF refining: lime and fluorite are added to the molten steel obtained in step (1) to perform white slag refining operation, keeping the slag white, blowing argon throughout the process, the argon pressure is 0.8 MPa, weak stirring is performed, the slag surface is kept slightly turned over and not exposed, the inlet temperature is 1540°C, the outlet temperature is 1630°C, and the temperature and composition are finely adjusted. The composition standards are C: 0.15%, Si: 0.14%, Al: 0.025%;

[0033] (3) RH refining: The arrival temperature of the molten steel obtained in step (2) is 1615°C, and titanium iron (FeTi30-A) is added to adjust the composition of the molten steel, and the composition control standard is Ti: 0.014%; the molten steel is vacuum treated, the vacuum degree is 200 Pa, the pressure holding time is 15 minutes, and the pure degassing time is 8 minutes; the ladle is soft-blown with argon gas for 15 minutes, and finally calcium aluminum wire is fed for calcium treatment, the feeding amount is 1.5 m / t, the feeding speed is 150 m / min, and the molten steel outlet temperature is controlled to be 1575°C;

[0034] (4) Continuous casting: The molten steel obtained in step (3) is cast on a 300 mm × 2300 mm cross-section continuous casting machine, with protective casting adopted throughout the process, the superheat of the tundish is 20-35° C., the casting speed is controlled at 1.15 m / min, and the continuous casting slab is directly hot-transferred after cutting;

[0035] (5) Slab heating: The continuous casting slab obtained in step (4) is placed in a heating furnace with an oxygen content of 3.3% for heating and then taken out of the furnace. The furnace temperature is controlled at 1243° C. and the total time in the furnace is 182 min.

[0036] (6) Rough dephosphorization: The slab heated in step (5) is subjected to rough dephosphorization by superimposing large-flow and small-flow descaling. The large-flow descaling water pressure is 19.5 MPa and the flow rate is 440 m 3 / h, small flow descaling water pressure is 22.5MPa, flow rate is 150m 3 / h, until the furnace-generated iron oxide scale on the surface of the slab is completely removed, and the intermediate slab is obtained;

[0037] (7) Finish rolling: the intermediate billet obtained in step (6) is sent to a furnace coil mill for finish rolling, the rolling passes are 7, the start rolling temperature of the finish rolling is controlled at 1084°C, and the final rolling temperature is controlled at 827°C;

[0038] (8) Secondary descaling: During finishing rolling, descaling between stands is turned on to reduce the formation of iron oxide scale. The descaling passes are 1, 2, 3, 5, 6, and 7 of rolling. Among them, high-flow descaling is used for finishing 1, 2, 3, and 5. The descaling water pressure is 19.5 MPa and the flow rate is 440 m 3 / h, small flow rate descaling is used in the 6th and 7th passes of finishing rolling, the water pressure is 22.5MPa, and the flow rate is 150m 3 / h;

[0039] (9) Coiling: The finished rolled slab obtained in step (8) is placed in a coiling furnace for coiling, with the temperature before the machine being 896°C and the temperature after the machine being 879°C, to obtain thin-gauge AH36 steel with a thickness of less than 8 mm.

[0040] The surface quality of the AH36 steel obtained above was analyzed. Figure 2 It can be seen that AH36 steel has a smooth surface, good quality and meets the use standards.

[0041] Example 2

[0042] A thin gauge AH36 steel, whose chemical composition by weight percentage is: C: 0.16%, Si: 0.13%, S: 0.002%, P: 0.015%, Mn: 1.36%, Al: 0.026%, Cr: 0.03%, Nb: 0.017%, V: 0.01%, Ti: 0.013%, Cu: 0.02%, Ni: 0.01%, and the balance is iron and unavoidable impurity elements. The process flow is: converter smelting → LF refining → RH refining → continuous casting → slab heating → rough descaling → finishing rolling → secondary descaling → coiling, and the specific steps are as follows:

[0043] (1) Converter smelting: molten iron is added to a 100t converter for smelting, the final temperature is 1640°C, the final carbon content of the converter is 0.08%, and deoxidation and alloying are performed during the converter tapping process. The addition amounts of each component are as follows: silicon manganese alloy (FeMn68Si18): 9.4kg / t, high carbon ferromanganese (FeMn68C7.0): 11.79kg / t, ferroniobium (FeNb60-B): 0.3kg / t, ferrotitanium (FeTi30-A): 0.9kg / t, aluminum ferromanganese (FeMnAl55): 2.6kg / t, aluminum particles 0.6kg / t, aluminum wire Φ13: 1m / t;

[0044] (2) LF refining: lime and fluorite are added to the molten steel obtained in step (1) to perform white slag refining operation, keeping the slag white, blowing argon throughout the process, the argon pressure is 0.8 MPa, weak stirring is performed, the slag surface is kept slightly turned over and not exposed, the inlet temperature is 1540°C, the outlet temperature is 1630°C, and the temperature and composition are finely adjusted. The composition standards are C: 0.16%, Si: 0.13%, Al: 0.026%;

[0045] (3) RH refining: The temperature of the molten steel obtained in step (2) is 1615°C, and titanium iron (FeTi30-A) is added to adjust the composition of the molten steel, and the composition control standard is Ti: 0.013%; the molten steel is vacuum treated, the vacuum degree is 200 Pa, the pressure holding time is 15 minutes, and the pure degassing time is 8 minutes; the ladle is soft-blown with argon gas for 15 minutes, and finally calcium aluminum wire is fed for calcium treatment, the feeding amount is 1.5 m / t, the feeding speed is 150 m / min, and the molten steel outlet temperature is controlled to be 1575°C;

[0046] (4) Continuous casting: The molten steel obtained in step (3) is cast on a 230 mm × 2450 mm cross-section continuous casting machine, with protective casting adopted throughout the process, the superheat of the tundish is 20 to 35° C., the casting speed is controlled at 1.2 m / min, and the continuous casting slab is directly hot-transferred after cutting;

[0047] (5) Slab heating: The continuous casting slab obtained in step (4) is placed in a heating furnace with an oxygen content of 3.3% for heating and then taken out of the furnace. The furnace temperature is controlled at 1246° C. and the total time in the furnace is 175 min.

[0048] (6) Rough dephosphorization: The slab heated in step (5) is subjected to rough dephosphorization by superimposing large-flow and small-flow descaling. The large-flow descaling water pressure is 22 MPa and the flow rate is 450 m 3 / h, small flow descaling water pressure is 23MPa, flow rate is 160m 3 / h, until the furnace-generated iron oxide scale on the surface of the slab is completely removed, and the intermediate slab is obtained;

[0049] (7) Finish rolling: the intermediate billet obtained in step (6) is sent to a furnace coil mill for finish rolling, the rolling passes are 7, the start rolling temperature of the finish rolling is controlled at 1081° C., and the final rolling temperature is controlled at 831° C.;

[0050] (8) Secondary descaling: During finishing rolling, descaling between stands is turned on to reduce the formation of iron oxide scale. The descaling passes are 1, 2, 3, 5, 6, and 7 of rolling. Among them, high-flow descaling is used for finishing 1, 2, 3, and 5. The descaling water pressure is 22 MPa and the flow rate is 450 m 3 / h, small flow descaling is used in the 6th and 7th passes of finishing rolling. The small flow descaling water pressure is 23MPa and the flow rate is 160m 3 / h;

[0051] (9) Coiling: The finished rolled slab obtained in step (8) is placed in a coiling furnace for coiling, with the temperature before the machine being 890° C. and the temperature after the machine being 880° C., to obtain thin-gauge AH36 steel with a thickness of less than 8 mm.

[0052] The surface quality of the AH36 steel obtained above was analyzed. Figure 3 It can be seen that AH36 steel has a smooth surface, good quality and meets the use standards.

[0053] Example 3

[0054] A thin gauge AH36 steel, whose chemical composition by weight percentage is: C: 0.17%, Si: 0.14%, S: 0.003%, P: 0.015%, Mn: 1.34%, Al: 0.024%, Cr: 0.03%, Nb: 0.016%, V: 0.01%, Ti: 0.015%, Cu: 0.01%, Ni: 0.01%, the balance is iron and unavoidable impurity elements. The process flow is: converter smelting → LF refining → RH refining → continuous casting → slab heating → rough descaling → finishing rolling → secondary descaling → coiling, the specific steps are as follows:

[0055] (1) Converter smelting: molten iron is added to a 100t converter for smelting, the final temperature is 1640°C, the final carbon content of the converter is 0.08%, and deoxidation and alloying are performed during the converter tapping process. The addition amounts of the components are as follows: silicon manganese alloy (FeMn68Si18): 9.8kg / t, high carbon ferromanganese (FeMn68C7.0): 12.15kg / t, ferroniobium (FeNb60-B): 0.26kg / t, ferrotitanium (FeTi30-A): 1.2kg / t, aluminum ferromanganese (FeMnAl55): 2.4kg / t, aluminum particles 0.45kg / t, aluminum wire Φ13: 0.9m / t;

[0056] (2) LF refining: lime and fluorite are added to the molten steel obtained in step (1) to perform white slag refining operation, keeping the slag white, blowing argon throughout the process, the argon pressure is 0.75 MPa, weak stirring is performed, the slag surface is kept slightly turned over and not exposed, the inlet temperature is 1540°C, the outlet temperature is 1630°C, and the temperature and composition are finely adjusted. The composition standards are C: 0.17%, Si: 0.14%, Al: 0.024%;

[0057] (3) RH refining: The arrival temperature of the molten steel obtained in step (2) is 1615°C, and titanium iron (FeTi30-A) is added to adjust the composition of the molten steel, and the composition control standard is Ti: 0.015%; the molten steel is vacuum treated, the vacuum degree is 200 Pa, the pressure holding time is 15 minutes, and the pure degassing time is 8 minutes; the ladle is soft-blown with argon gas for 15 minutes, and finally calcium aluminum wire is fed for calcium treatment, the feeding amount is 1.4 m / t, the feeding speed is 150 m / min, and the molten steel outlet temperature is controlled to be 1575°C;

[0058] (4) Continuous casting: The molten steel obtained in step (3) is cast on a 230 mm × 1850 mm cross-section continuous casting machine, with protective casting adopted throughout the process, the superheat of the tundish is 20 to 35° C., the casting speed is controlled at 1.20 m / min, and the continuously cast slab is directly hot-transferred after being cut;

[0059] (5) Slab heating: The continuous casting slab obtained in step (4) is placed in a heating furnace with an oxygen content of 3.3% and heated before being taken out of the furnace. The furnace temperature is controlled at 1241° C. and the total furnace time is 190 min.

[0060] (6) Rough dephosphorization: The slab heated in step (5) is subjected to rough dephosphorization by superimposing large-flow and small-flow descaling. The large-flow descaling water pressure is 22.5 MPa and the flow rate is 455 m 3 / h, small flow descaling water pressure is 23MPa, flow rate is 160m 3 / h, until the furnace-generated iron oxide scale on the surface of the slab is completely removed, and the intermediate slab is obtained;

[0061] (7) Finish rolling: the intermediate billet obtained in step (6) is sent to a furnace coil mill for finish rolling, the rolling passes are 7, the start rolling temperature of the finish rolling is controlled at 1082° C., and the final rolling temperature is controlled at 838° C.;

[0062] (8) Secondary descaling: During finishing rolling, descaling between stands is turned on to reduce the formation of iron oxide scale. The descaling passes are 1, 2, 3, 5, 6, and 7 of rolling. Among them, high-flow descaling is used for finishing 1, 2, 3, and 5. The descaling water pressure is 22.5 MPa and the flow rate is 455 m 3 / h, small flow rate descaling is used in the 6th and 7th passes of finishing rolling, the descaling water pressure is 23MPa, and the flow rate is 160m3 / h;

[0063] (9) Coiling: The finished rolled slab obtained in step (8) is placed in a coiling furnace for coiling, with the temperature before the machine being 895°C and the temperature after the machine being 877°C, to obtain thin-gauge AH36 steel with a thickness of less than 8 mm.

[0064] The surface quality of the AH36 steel obtained above was analyzed. Figure 4 As shown, AH36 steel has a smooth surface, good quality and meets the use standards.

Claims

1. A method for controlling oxide scale defects on the surface of thin-gauge AH36 steel, comprising: Converter smelting → LF refining → RH refining → continuous casting → slab heating → rough descaling → finishing rolling → secondary descaling → coiling, which is characterized in that the Si content is reduced in the converter smelting process, the Si content is 0.12-0.15% by weight, and rough phosphorus removal is carried out by superimposing large flow and small flow descaling before finishing rolling, and secondary descaling is carried out by odd + even number passes in combination during finishing rolling.

2. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 1 is characterized in that: The method comprises the following steps: (1) Slab composition control: Continuously cast slabs are obtained through "converter smelting → LF refining → RH refining → continuous casting", in which the Si content is reduced during the converter smelting process; (2) Slab heating: the continuous casting slab obtained in step (1) is placed in a heating furnace with an oxygen content of less than 3.5% for heating and then taken out of the furnace; (3) Rough dephosphorization: The slab heated in step (2) is subjected to rough dephosphorization by superimposing large-flow and small-flow descaling processes to achieve the standard of completely removing the furnace-born iron oxide scale on the surface of the slab, thereby obtaining an intermediate slab; (4) Finish rolling: The intermediate billet obtained in step (3) is subjected to finish rolling, with the number of rolling passes being 7 to 9; (5) Secondary descaling: During finishing rolling, descaling between stands is turned on, and secondary dephosphorization is performed by combining odd and even passes; (6) Coiling: The finished rolled slab obtained in step (5) is coiled to obtain thin-gauge AH36 steel with a thickness of less than 8 mm.

3. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2 is characterized in that: The chemical composition of the slab in step (1) is as follows by weight: C: 0.15-0.20%, Si: 0.12-0.15%, S: 0.001-0.004%, P: 0.010-0.020%, Mn: 1.10-1.50%, Al: 0.020-0.050%, Cr: ≤0.03%, Nb: 0.015-0.020%, V: ≤0.01%, Ti: 0.010-0.015%, Cu: ≤0.02%, Ni: ≤0.01%, and the remainder is iron and unavoidable impurity elements.

4. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2 is characterized in that: The furnace temperature in step (2) is controlled at 1230-1250° C., and the total furnace time is ≤190 min.

5. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2, characterized in that: The method of superimposing the large flow rate and small flow rate descaling in step (3) means that during the dephosphorization process, the large flow rate and small flow rate descaling nozzles are opened simultaneously to perform slab dephosphorization.

6. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2, characterized in that: The high-flow descaling water pressure in step (3) is 19-23 MPa, and the flow rate is 430-460 m 3 / h; the small flow descaling water pressure is 22-24MPa, and the flow rate is 140-165m 3 / h.

7. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2, characterized in that: In step (4), the start rolling temperature of the finishing rolling is controlled at 1080-1100°C, and the final rolling temperature is controlled at 820-840°C.

8. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2, characterized in that: The descaling passes between the stands in step (5) are 1, 2, 3, 5, 6, and 7 of rolling, 1, 2, 3, and 5 passes use large flow rate dephosphorization, and 6 and 7 passes use small flow rate descaling.

9. The method for controlling the iron oxide scale defects on the surface of AH36 steel according to claim 2, characterized in that: The coiling temperature in step (6) is 850-900°C.

10. Thin gauge AH36 steel produced according to the method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for removing bright trace on surface of strip steel

    CN102921750A

  • Control method for eliminating pockmark defect on surface of hot-rolling ship board

    CN103480655A

  • Thin gauge steel plate used for marine engineering and preparation method thereof

    CN105779865A

  • Method for controlling oxide scale of rolled cold-rolled base material

    CN114054515A

  • Heat treatment production method of thin-gauge series wear-resistant steel plate

    CN116219122A

Cited By

  • Scale control method suitable for hot rolling SPHC

    CN119857721A

  • Method for controlling oxide scale on surface of hot-rolled strip steel

    CN119972822A