Blast furnace tapping main channel castable and preparation method thereof
By using composite graphite microsphere particles and magnesium carbide, boron carbide and aluminum metal powder in the blast furnace iron discharge castable, the problems of insufficient amount of carbon materials and narrow anti-oxidation temperature range are solved, and the resistance is improved Erosion, thermal shock resistance and high temperature resistance extend service life.
Patent Information
- Application Number
- CN202410958886.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The amount of carbon material added in the castable material of the existing blast furnace discharge main groove is relatively low, the amount of water is too much, and the oxidation temperature range is narrow, resulting in insufficient erosion resistance, thermal shock resistance and high temperature resistance.
The composite graphite microsphere particles and magnesium carbide, boron carbide, and metal aluminum powder are used as carbon materials and antioxidants to form C@MgO@Al2O3@SiO2 microsphere particles through wet granulation to improve the dispersion of carbon materials. and antioxidant properties, and produce magnesium aluminum spinel and mullite under high temperature conditions, enhancing the high temperature and thermal shock resistance of the castable material.
It significantly improves the corrosion resistance, thermal shock stability and oxidation resistance of the castable material, reduces the amount of water distribution, enhances the high temperature resistance and flexural strength, and extends the service life.
Smart Images

Figure BDA0004949715090000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a blast furnace tapping main ditch castable and a preparation method thereof. Background Art
[0002] The blast furnace tapping ditch is the channel through which the molten iron and slag flow in the blast furnace. It is divided into the main ditch, branch ditch and slag ditch. The main ditch is the common channel for the high-temperature slag-iron mixture flowing out of the blast furnace. A slag skimmer is designed at the rear of the main ditch. The molten iron in the main ditch enters the branch ditch from the bottom of the slag skimmer, and the slag in the main ditch enters the slag ditch from the top of the slag skimmer beam. The main ditch is the most important and has the worst operating environment. It not only has to withstand the erosion of high-temperature molten iron, but also the erosion of high-temperature slag and thermal shock damage caused by sudden temperature changes. With the development of steel smelting technology, the requirements for the materials of the blast furnace tapping main ditch are getting higher and higher. The material laid in the tapping ditch is called castable, which is a refractory material.
[0003] In order to resist the erosion of molten iron and slag, carbon materials need to be added to the castable. Carbon has the characteristics of not being easily wetted by molten iron and slag, small thermal expansion coefficient and high thermal conductivity. The introduction of carbon materials can improve the erosion resistance and thermal shock stability of the iron outlet ditch. However, the addition of carbon materials will also bring new problems, mainly including: (1) Due to the poor water wettability of carbon, it is easy to float in the castable and difficult to disperse evenly. Therefore, the amount of carbon material added in the prior art is relatively low, generally not exceeding 4%; (2) After the carbon material is introduced into the castable, in order to achieve appropriate fluidity, more water needs to be added to improve the construction performance. Generally, the amount of water added is more than 5% of the total mass of the castable. However, after adding more water, the time required for the castable to dry will be greatly increased; (3) Carbon materials are easily oxidized and lost in high-temperature use environments, which leads to reduced corrosion resistance, thermal shock resistance and high temperature resistance of the castable. In order to effectively play the role of carbon materials, antioxidants need to be added to the castable. However, the antioxidants in the prior art generally have a narrow anti-oxidation temperature range, which results in the carbon material's effective role not being better played.
[0004] Chinese patent CN117247272A discloses an anti-oxidation blast furnace iron channel castable and its preparation method, wherein the raw material composition mass percentage is: 10.5-12% of 15-8mm brown corundum, 14.5-16% of 8-5mm brown corundum, 10-12% of 5-3mm brown corundum, 10-11% of 3-1mm brown corundum, 9-10% of 3-1mm dense corundum, 4-5% of 1-0mm dense corundum, 11-13% of 1-0mm silicon carbide, 325 mesh carbon Silicon dioxide is 9-10%, aluminum oxide powder is 4-6%, silicon powder is 1.5-2.5%, high alumina cement is 1-1.5%, ρ-Al2O3 is 1-1.5%, andalusite is 0.5-1%, spherical asphalt is 2-2.5%, carbon black is 0.5-1%, boron carbide is 0.2-0.4%, molybdenum strontium powder is 0.05-0.1%, metal silicon powder is 1.5-2.5%, metal aluminum powder is 0.02-0.04%, organic fiber is 0.04-0.07%, and water reducer is 0.1-0.3%. In the invention, a compound of spherical asphalt and modified carbon black is used as the carbon material, and molybdenum strontium powder, metal silicon powder and metal aluminum powder are used as antioxidants; wherein, the modified carbon black is obtained by impregnating the surface of carbon black with trimethyl aluminum, so that trimethyl aluminum reacts with the hydroxyl or carbonyl group on the surface of carbon black to form a chemical bond. The blast furnace iron ditch castable produced by this invention improves its antioxidant properties, thereby improving the performance and service life of the castable, but the maximum amount of carbon material added to the castable can only reach 3.5%, and the antioxidant temperature range is narrow, and the antioxidant effect is only good above 1000°C. Summary of the invention
[0005] In view of the problems in the prior art that the carbon material in the blast furnace iron ditch castable cannot effectively play its role, the added amount is low, the required amount of water is too much, and the anti-oxidation temperature range in the castable is narrow, the present invention provides a blast furnace iron-outlet main ditch castable to solve the above problems, thereby improving the corrosion resistance, thermal shock stability and oxidation resistance of the iron-outlet main ditch castable, and having excellent pressure resistance.
[0006] The present invention achieves the above object through the following technical solutions:
[0007] The invention provides a blast furnace tapping main channel castable, comprising the following raw materials in parts by mass: 45-55 parts of dense corundum, 12-25 parts of white corundum, 12-20 parts of silicon carbide, 3-6 parts of α-Al2O3 powder, 2-6 parts of ρ-Al2O3 powder, 5-10 parts of composite graphite particles, 0.5-0.8 parts of aluminum nitride powder, 1-5 parts of antioxidant, 0.1-0.3 parts of explosion-proof fiber, and 0.1-0.5 parts of water reducer; the composite graphite particles are C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursors formed by wet granulation of graphite, magnesium sol, aluminum sol and silica sol, and calcined in an inert atmosphere to form C@Mg(OH)2@Al(OH)3@SiO2 microsphere particles; the antioxidant is a compound of magnesium carbide, boron carbide and aluminum powder.
[0008] Carbon materials can enhance the ability to resist slag erosion and are an indispensable raw material for the iron trough castable. However, conventional carbon materials have poor wettability with water, resulting in uneven dispersion in the matrix, so that the amount added is low and the amount of water added is high. The present invention forms C@MgO@Al2O3@SiO2 microsphere particles, i.e., composite graphite particles, after wet granulation and calcination. On the one hand, the dispersibility and wettability of graphite with water are greatly improved, thereby increasing the amount of carbon added, which is more conducive to improving the ability of the castable to resist slag erosion. On the other hand, in the subsequent production process of the main iron channel castable, Al2O3 in the C@MgO@Al2O3@SiO2 microsphere particles reacts with MgO and SiO2 in situ under high temperature conditions to generate magnesia-alumina spinel and mullite, which improve the high temperature strength and thermal shock resistance of the castable; at the same time, the in-situ generated magnesia-alumina spinel and mullite have fine particle sizes, which are more conducive to improving the slag erosion resistance of the castable than the "pre-synthesized" magnesia-alumina spinel and mullite. In addition, there is a volume micro-expansion effect in the process of in-situ generation of magnesia-alumina spinel and mullite, which is conducive to improving the density of the castable, thereby further improving the erosion resistance and high temperature strength of the castable.
[0009] Carbon materials are easy to oxidize, and generally, antioxidants need to be added to the iron ditch castable to inhibit the oxidation of carbon. The present invention uses a compound of magnesium carbide, boron carbide, and metal aluminum powder as an oxidant; the antioxidant reacts with oxygen before carbon at high temperatures, wherein magnesium carbide has a good antioxidant effect at 600-800°C, boron carbide has a good antioxidant effect at 800-1000°C, and aluminum powder has a good antioxidant effect at 1000°C; the antioxidant formed by the compound of the three has a good antioxidant effect in the entire high temperature range.
[0010] Furthermore, the mass ratio of graphite, Mg(OH)2, Al(OH)3 and SiO2 in the C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor is 1:(0.1~0.2):(0.3~0.5):(0.15~0.25); preferably 1:(0.1~0.2):(0.4~0.5):(0.2~0.25).
[0011] Furthermore, the composite graphite particles are prepared by a method comprising the following steps:
[0012] (P1) mixing graphite, magnesium sol, aluminum sol and silica sol to form a mixed slurry;
[0013] (P2) granulating the mixed slurry by a wet process to obtain a C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor;
[0014] (P3) The C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor is calcined under an inert atmosphere to obtain C@MgO@Al2O3@SiO2 microsphere particles, i.e., composite graphite particles.
[0015] Furthermore, in step (P1), the particle size D50 of the magnesium sol is 10-60 nm, and its solid content is 20%-40%, the D50 of the aluminum sol is 10-60 nm, and its solid content is 20%-40%, and the D50 of the silica sol is 10-60 nm, and its solid content is 20%-40%;
[0016] Furthermore, the conditions for the wet granulation in step (P2) are: granulation is carried out by a wet granulator, the inlet temperature of the wet granulator is 150-250°C, the outlet temperature is 70-120°C, and the rotation speed is 1500-3000rpm; the inert atmosphere is at least one of nitrogen, argon, and helium.
[0017] Furthermore, the calcination in step (P3) is performed at 300-500° C. for 3-6 hours.
[0018] Furthermore, in the antioxidant, the mass ratio of magnesium carbide, boron carbide and aluminum powder is 1:(1-3):(1-2); preferably 1:(2-3):(1-2).
[0019] Furthermore, the particle size of the dense corundum is 1 to 8 mm; the particle size of the white corundum is 0.1 to 3 mm; and the particle size of the silicon carbide is 100 to 400 meshes.
[0020] Furthermore, the dense corundum gradation meets the following requirements: 15-25wt% of particles with a particle size of 8-5mm, 40-60wt% of particles with a particle size of 5-3mm, and 20-40wt% of particles with a particle size of 3-1mm; the white corundum gradation meets the following requirements: 60-80wt% of particles with a particle size of 3-1mm, and 20-40wt% of fine powder with a particle size of 1-0.1mm; the silicon carbide gradation meets the following requirements: 60-75wt% of fine powder with a particle size of 100-200 mesh, and 25-40wt% of micro powder with a particle size of 200-400 mesh.
[0021] Furthermore, in the dense corundum and white corundum, Al2O3≥99wt%, Fe2O3≤0.1wt%, SiO2≤0.1wt%; in the silicon carbide, SiC≥97wt%, SiO2≤0.4wt%, Fe2O3≤0.3wt%.
[0022] Furthermore, the particle size D50 of the α-Al2O3 powder is 1 to 6 μm, and the Al2O3 in the α-Al2O3 powder is ≥ 99.0 wt%.
[0023] Furthermore, the particle size D50 of the ρ-Al2O3 powder is 1 to 6 μm, and the Al2O3 in the ρ-Al2O3 powder is ≥ 98.0 wt%.
[0024] Furthermore, the particle size D50 of the composite graphite particles is 15 to 60 μm; the particle size D50 of the graphite is 1 to 6 μm; and the graphite is at least one of artificial graphite, natural graphite, and graphitized mesophase carbon microspheres.
[0025] Furthermore, the particle size D50 of the aluminum nitride powder is 200-400 mesh. The aluminum nitride powder decomposes when it meets water, producing hydrogen and aluminum oxide, which consumes the excess water in the raw materials to achieve the purpose of quick drying; at the same time, the released ammonia forms micropores in the matrix, and another part of the water vapor will be discharged along these pore channels, further promoting quick drying.
[0026] Furthermore, in the antioxidant, the particle size of magnesium carbide is 200-400 meshes, the particle size of boron carbide is 200-400 meshes, and the particle size of aluminum powder is 200-400 meshes.
[0027] Furthermore, the anti-burst fiber is made of organic fiber, such as nylon, polyethylene fiber, polypropylene fiber, with a melting point of 90-160° C., a diameter of 4-8 μm, and a length of 8-15 mm.
[0028] Based on the maximum packing density theory, the different particle sizes of the component raw materials can be packed most densely in the best proportion, that is, the gaps between the stacked millimeter-sized particles (compact corundum, white corundum) are filled with micron-sized particles (silicon carbide, composite graphite particles, aluminum nitride powder), and the gaps between the stacked micron-sized particles are filled with ultrafine powders (α-Al2O3 powder, ρ-Al2O3 powder). In this way, the whole system is tightly wrapped to form a complete and dense matrix structure, thereby improving the structural strength of the castable.
[0029] Furthermore, the water reducer is a polycarboxylate water reducer and / or sodium hexametaphosphate.
[0030] In a second aspect, the present invention also provides a method for preparing the above-mentioned blast furnace main ditch castable, comprising the following steps:
[0031] (S1) adding silicon carbide, α-Al2O3 powder, ρ-Al2O3 powder, composite graphite particles, aluminum nitride powder, and an antioxidant into a container and mixing and stirring to obtain a mixed fine material;
[0032] (S2) adding dense corundum and white corundum into another container and mixing and stirring to obtain mixed granules;
[0033] (S3) Under stirring, the mixed fine material obtained in (S1) is added to the mixed granular material obtained in (S2), and then explosion-proof fiber and water reducing agent are added for mixing and stirring to obtain a blast furnace main ditch castable.
[0034] Furthermore, the stirring in step (S1) is carried out at a speed of 500 to 1000 r / min for 30 to 60 min; the stirring in step (S2) is carried out at a speed of 200 to 400 r / min for 10 to 30 min; and the stirring in step (S3) is carried out at a speed of 200 to 400 r / min for 10 to 30 min.
[0035] In a third aspect, the present invention further provides a construction method for adding water to the main trough castable, wherein the amount of water added is 2 to 3.5% of the total mass of the main trough castable.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1) In order to improve the anti-corrosion ability of the castable by molten iron and iron slag, carbon materials such as graphite and coke need to be added to the castable; however, conventional carbon materials such as graphite and coke have poor wettability with water, resulting in a low amount of addition and uneven dispersion in the matrix. The present invention uses composite graphite microsphere particles as carbon materials, that is, C@MgO@Al2O3@SiO2 microsphere particles as carbon materials, which greatly improves the dispersibility of graphite and its wettability with water, thereby increasing the amount of carbon added and reducing the amount of water added. The amount of composite graphite particles added in the present invention is 5-10%, which is more conducive to improving the anti-slag erosion ability of the castable; at the same time, the amount of water required during the pouring construction stage is relatively small, only 2-3.5% of the total mass of the castable of the main trough for iron tapping.
[0038] 2) In the subsequent production process of the main iron channel castable, under high temperature conditions, Al2O3 in the composite graphite particles C@MgO@Al2O3@SiO2 microspheres reacts with MgO and SiO2 in situ to generate magnesium aluminum spinel and mullite, which improve the high temperature strength and thermal shock resistance of the castable; at the same time, the in-situ generated magnesium aluminum spinel and mullite have fine particles, which are more conducive to the improvement of the castable's slag erosion resistance than the "pre-synthesized" magnesium aluminum spinel and mullite. In addition, there is a volume micro-expansion effect in the process of in-situ generation of magnesium aluminum spinel and mullite, which is conducive to improving the compactness of the castable, and further improving its slag erosion resistance and high temperature strength. That is, using C@MgO@Al2O3@SiO2 microspheres as carbon materials not only plays the role of carbon materials and improves the castable's erosion resistance; it also improves the castable's high temperature strength and thermal shock resistance.
[0039] 3) The present invention adopts a compound of magnesium carbide, boron carbide and metallic aluminum powder as an antioxidant, giving full play to the advantages of each component at different temperature stages; the antioxidant reacts with oxygen before carbon at high temperatures, wherein magnesium carbide has a good antioxidant effect at 600-800°C, boron carbide has a good antioxidant effect at 800-1000°C, and aluminum powder has a good antioxidant effect above 1000°C; the composite antioxidant formed by the compound of the three ensures that the castable has a good antioxidant effect within the entire high temperature range.
[0040] 4) Aluminum nitride powder decomposes when it comes into contact with water, generating hydrogen and aluminum oxide, which consumes the excess water in the raw materials to achieve the purpose of quick drying; at the same time, the released ammonia forms micropores in the matrix, and another part of the water vapor will be discharged along these pore channels.
[0041] 5) The main components of the castable for the main ditch of the iron ditch of the present invention are alumina and silicon carbide. Dense corundum, white corundum, α-Al2O3 powder and ρ-Al2O3 are the main sources of alumina; among them, dense corundum and white corundum have low porosity and high hardness, which can improve the castable's resistance to iron slag penetration; α-Al2O3 powder and ρ-Al2O3 can improve the fluidity of the castable, thereby improving the construction performance. At the same time, ρ-Al2O3 has the ability of spontaneous hydration at room temperature, acts as a binder, and in the subsequent production process of the main iron ditch castable, no low melting point phase is generated at the high temperature stage, so that the castable has better slag resistance. Silicon carbide has the characteristics of high hardness, high strength, low thermal expansion coefficient and high thermal conductivity, which can improve the sintering strength and slag resistance of the castable. In addition, based on the bulk density theory, the raw material particle size and ratio are preferably selected so that the entire system of the prepared castable is tightly wrapped to form a complete and dense matrix structure.
[0042] 6) In summary, the main ditch castable of the iron outlet ditch of the present invention has excellent flexural strength, compressive strength and low linear change rate both at low temperature and high temperature stages; its flexural strength in the cold state after firing at 1400℃×3h is above 12Mpa, its compressive strength is above 64Mpa, its linear change rate is lower than +0.3%, and its flexural strength in the hot state at 1400℃×0.5h is above 4.2Mpa. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with specific embodiments.
[0044] Unless otherwise specified in the following examples, the reagents and materials described can be obtained from commercial sources.
[0045] Unless otherwise specified, the “parts” in the embodiments of the present invention are parts by mass, and the “%” are percentages by mass.
[0046] The magnesium sol was selected from Hebei Meixi Biological Co., Ltd., with a particle size D50 of 40 nm and a solid content of 30%.
[0047] The aluminum sol was selected from LJ-030 produced by Yangzhou Zhongtianli New Materials Co., Ltd., with a particle size D50 of 30 nm and a solid content of 30%.
[0048] The silica sol was selected from SW15-30 / 1 of Zhejiang Delixin Micro-Nano Technology Co., Ltd., with a particle size D50 of 15 nm and a solid content of 30%.
[0049] The graphite was selected from Qingdao Yuchen Graphite Co., Ltd., and the particle size D50 was 4.6 μm.
[0050] The particle size D50 of α-Al2O3 powder is 5.1μm, the particle size D50 of ρ-Al2O3 powder is 4.7μm, the particle size of aluminum nitride powder is 300 mesh, the particle size of magnesium carbide is 325 mesh, the particle size of boron carbide is 325 mesh, and the particle size of aluminum powder is 325 mesh.
[0051] The explosion-proof fiber is selected from the polyethylene fiber of Shandong Oude Chemical Fiber Products Co., Ltd., with a melting point of 105°C, a diameter of 5-6μm, and a length of 10mm.
[0052] Preparation of composite graphite particles
[0053] Preparation Example 1
[0054] (P1) 1000 g of graphite, 333 g of magnesium sol with a solid content of 30%, 1000 g of aluminum sol with a solid content of 30%, and 500 g of silica sol with a solid content of 30% were mixed (i.e., the mass ratio of graphite, Mg(OH)2, Al(OH)3, and SiO2 was 1:0.1:0.3:0.15), and then stirred and dispersed in a high-speed disperser for 5 hours to form a mixed slurry;
[0055] (P2) The mixed slurry was granulated by a wet granulator to obtain a C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor with a particle size D50 of 31.2 μm; the inlet temperature of the wet granulator was 200°C, the outlet temperature was 90°C, and the rotation speed was 2100 rpm;
[0056] (P3) The C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor was calcined at 350°C for 4 h under a nitrogen atmosphere to obtain C@MgO@Al2O3@SiO2 microsphere particles, i.e., composite graphite particles a1, with a particle size D50 of 31.2 μm.
[0057] Preparation Example 2
[0058] The rest is the same as Preparation Example a1, except that the amounts of graphite, magnesium sol, aluminum sol and silica sol in step (P1) are: 1000 g graphite, 500 g magnesium sol with a solid content of 30%, 1333 g aluminum sol with a solid content of 30%, 667 g silica sol with a solid content of 30% (i.e., the mass ratio of graphite, Mg(OH)2, Al(OH)3 and SiO2 is 1:0.15:0.4:0.2), and the particle size D50 of the obtained composite graphite particles a2 is 30.5 μm.
[0059] Preparation Example 3
[0060] The rest is the same as Preparation Example a1, except that the amounts of graphite, magnesium sol, aluminum sol and silica sol in step (P1) are: 1000 g graphite, 667 g magnesium sol with a solid content of 30%, 1667 g aluminum sol with a solid content of 30%, 833 g silica sol with a solid content of 30% (i.e., the mass ratio of graphite, Mg(OH)2, Al(OH)3 and SiO2 is 1:0.2:0.5:0.25), and the particle size D50 of the obtained composite graphite particles a3 is 31.6 μm.
[0061] Comparative Preparation Example 1
[0062] The rest is the same as Preparation Example a1, except that, in step (P1), aluminum sol is not used, and only graphite, magnesium sol and silica sol are used; the amounts of graphite, magnesium sol and silica sol are: 1000g graphite, 833g magnesium sol with a solid content of 30%, and 1000g silica sol with a solid content of 30%; the particle size D50 of the obtained composite graphite particles b is 31.3μm (the C content in the composite graphite particles b is the same as the C content of the composite graphite particles a1).
[0063] Example 1
[0064] A blast furnace iron tapping main ditch castable, comprising the following raw materials in parts by weight:
[0065] 50 parts of dense corundum, with a particle size of 3 to 5 mm;
[0066] 18 parts of white corundum, with a particle size of 1 to 3 mm;
[0067] 16 parts of silicon carbide, with a particle size of 200 mesh;
[0068] 4.5 parts of α-Al2O3 powder;
[0069] ρ-Al2O3 powder 4 parts;
[0070] The composite graphite particles a1 are 8 parts;
[0071] 0.6 parts of aluminum nitride powder;
[0072] 3 parts of antioxidant, including 1 part of magnesium carbide, 1 part of boron carbide, and 1 part of aluminum powder (i.e. 1:1:1);
[0073] 0.2 parts of explosion-proof fiber;
[0074] 0.3 parts of water reducing agent sodium hexametaphosphate.
[0075] The preparation method comprises the following steps:
[0076] (S1) adding silicon carbide, α-Al2O3 powder, ρ-Al2O3 powder, composite graphite particles, aluminum nitride powder, and an antioxidant into a container, and stirring at a speed of 600 r / min for 30 min to obtain a mixed fine material;
[0077] (S2) adding dense corundum and white corundum into another container, stirring at a speed of 200 r / min for 20 min to obtain mixed granules;
[0078] (S3) maintaining a stirring speed of 200 r / min, adding the mixed fine material obtained in (S1) to the mixed granular material obtained in (S2), and then adding explosion-proof fiber and water reducing agent and mixing and stirring at a speed of 200 r / min for 20 minutes to obtain the main ditch casting material of the iron ditch.
[0079] Example 2
[0080] The rest is the same as Example 1, except that in the raw material composition, the composite graphite particles a2 prepared in Preparation Example 2 are used to replace the composite graphite particles a1 prepared in Preparation Example 1.
[0081] Example 3
[0082] The rest is the same as Example 1, except that in the raw material composition, the composite graphite particles a3 prepared in Preparation Example 3 are used to replace the composite graphite particles a1 prepared in Preparation Example 1.
[0083] Example 4
[0084] The rest is the same as Example 2, except that in the raw material composition, the antioxidant is 3 parts, of which magnesium carbide is 0.6 parts, boron carbide is 1.2 parts, and aluminum powder is 1.2 parts (i.e. 1:2:2).
[0085] Example 5
[0086] The rest is the same as Example 2, except that in the raw material composition, the antioxidant is 3 parts, including 0.5 parts of magnesium carbide, 1.5 parts of boron carbide and 1 part of aluminum powder (i.e. 1:3:2).
[0087] Example 6
[0088] The rest of the examples are the same as in Example 1, except that in the raw material composition:
[0089] 50 parts of dense corundum, including 10 parts of particles with a particle size of 8 to 5 mm, 25 parts of particles with a particle size of 5 to 3 mm, and 15 parts of particles with a particle size of 3 to 1 mm;
[0090] 18 parts of white corundum, including 12 parts of particles with a particle size of 3 to 1 mm and 6 parts of fine powder with a particle size of 1 to 0.1 mm;
[0091] 16 parts of silicon carbide, including 11 parts of fine powder with a particle size of 200 mesh and 5 parts of micro powder with a particle size of 400 mesh;
[0092] The remaining components are the same as those in Example 1.
[0093] Example 7
[0094] The rest is the same as Example 1, except that the raw material composition is:
[0095] 45 parts of dense corundum, with a particle size of 3 to 5 mm;
[0096] 12 parts of white corundum, with a particle size of 1 to 3 mm;
[0097] 12 parts of silicon carbide, with a particle size of 0.1 to 1 mm;
[0098] α-Al2O3 powder 3 parts;
[0099] ρ-Al2O3 powder 2 parts;
[0100] The composite graphite particles a1 are 5 parts;
[0101] 0.5 parts of aluminum nitride powder;
[0102] 1 part of antioxidant, including 0.33 parts of magnesium carbide, 0.33 parts of boron carbide and 0.33 parts of aluminum powder;
[0103] 0.1 part of explosion-proof fiber;
[0104] 0.1 part of water reducing agent sodium hexametaphosphate.
[0105] Example 8
[0106] The rest is the same as Example 1, except that the raw material composition is:
[0107] 55 parts of dense corundum, with a particle size of 3 to 5 mm;
[0108] 25 parts of white corundum, with a particle size of 1 to 3 mm;
[0109] 20 parts of silicon carbide, with a particle size of 0.1 to 1 mm;
[0110] α-Al2O3 powder 6 parts;
[0111] ρ-Al2O3 powder 6 parts;
[0112] The composite graphite particles a1 are 10 parts;
[0113] 0.8 parts of aluminum nitride powder;
[0114] 5 parts of antioxidant, including 1.67 parts of magnesium carbide, 1.67 parts of boron carbide, and 1.67 parts of aluminum powder;
[0115] 0.3 parts of explosion-proof fiber;
[0116] 0.5 parts of water reducing agent sodium hexametaphosphate.
[0117] Comparative Example 1
[0118] The rest is the same as Example 1, except that 5.2 parts of graphite are used to replace 8 parts of composite graphite particles a1; the graphite content in 5.2 parts of graphite is equivalent to that in 8 parts of composite graphite particles a1.
[0119] Comparative Example 2
[0120] The rest is the same as Example 1, except that the composite graphite particles b prepared in Comparative Preparation Example 1 are used instead of the composite graphite particles a1.
[0121] Comparative Example 3
[0122] The rest is the same as Example 1, except that the antioxidant does not contain magnesium carbide, that is, 3 parts of the antioxidant, including 1.5 parts of boron carbide and 1.5 parts of aluminum powder.
[0123] Performance Testing
[0124] 3% of water was added to the main trough castables of the above embodiments and comparative examples, stirred at 200r / min for 10min, and vibrated on a vibration table to obtain a strip of 40mm×40mm×160mm in size. After 24h of mold curing in a normal temperature zone, the strip was demoulded, placed in a 110℃ oven for drying for 24h, kept at 1400℃ in a baking furnace under air atmosphere for 3h, and tested for hot flexural strength at 1400℃×0.5h. The performance test results are shown in Table 1.
[0125] Table 1 Performance test data
[0126]
[0127] It can be seen from Table 1 that the castables for the main ditch of the iron-outlet ditch prepared in Comparative Examples 1 to 3, although their bulk density, flexural strength and compressive strength can basically meet the use requirements at a low temperature of 110°C, when the temperature rises to 1400°C, their flexural strength and compressive strength are significantly lower. The castables for the main ditch of the iron-outlet ditch prepared in the embodiment of the present invention, whether in the low temperature or high temperature stage, are significantly better than the comparative examples in terms of bulk density, flexural strength, compressive strength and linear change rate; their flexural strength in the cold state after firing at 1400°C×3h is above 12Mpa, their compressive strength is above 64Mpa, their linear change rate is less than +0.3%, and their flexural strength in the hot state at 1400°C×0.5h is above 4.2Mpa. In summary, the castables for the main ditch of the iron-outlet ditch prepared in the present invention have excellent heat resistance, high strength and hardness, so that they have good corrosion resistance, thermal shock resistance and oxidation resistance, and thus can extend their service life.
[0128] The above description is only a preferred embodiment of the present invention and does not limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A blast furnace iron tapping main ditch castable, characterized in that: The invention comprises the following raw materials in parts by weight: 45-55 parts of dense corundum, 12-25 parts of white corundum, 12-20 parts of silicon carbide, 3-6 parts of α-Al2O3 powder, 2-6 parts of ρ-Al2O3 powder, 5-10 parts of composite graphite particles, 0.5-0.8 parts of aluminum nitride powder, 1-5 parts of antioxidant, 0.1-0.3 parts of explosion-proof fiber and 0.1-0.5 parts of water reducer; the composite graphite particles are C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursors formed by wet granulation of graphite, magnesium sol, aluminum sol and silica sol and calcined in an inert atmosphere to form C@MgO@Al2O3@SiO2 microsphere particles; the antioxidant is a compound of magnesium carbide, boron carbide and aluminum powder.
2. The blast furnace iron tapping main ditch castable according to claim 1, characterized in that: The mass ratio of graphite, Mg(OH)2, Al(OH)3 and SiO2 in the C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor is 1:(0.1~0.2):(0.3~0.5):(0.15~0.25); preferably 1:(0.1~0.2):(0.4~0.5):(0.2~0.25).
3. The blast furnace iron tapping main ditch castable according to claim 1, characterized in that: The composite graphite particles are prepared by a method comprising the following steps: (P1) mixing graphite, magnesium sol, aluminum sol and silica sol to form a mixed slurry; (P2) granulating the mixed slurry by a wet process to obtain a C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor; (P3) The C@Mg(OH)2@Al(OH)3@SiO2 microsphere precursor is calcined under an inert atmosphere to obtain C@MgO@Al2O3@SiO2 microsphere particles, i.e., composite graphite particles.
4. The blast furnace iron tapping main ditch castable according to claim 1, characterized in that: In the antioxidant, the mass ratio of magnesium carbide, boron carbide and aluminum powder is 1:(1-3):(1-2); preferably 1:(2-3):(1-2).
5. The blast furnace iron tapping main ditch castable according to claim 1, characterized in that: The particle size of the dense corundum is 1-8 mm; the particle size of the white corundum is 0.1-3 mm; and the particle size of the silicon carbide is 100-400 meshes.
6. The blast furnace iron-tapping main ditch castable according to claim 5, characterized in that: The dense corundum gradation meets the following requirements: 15-25wt% of particles with a particle size of 8-5mm, 40-60wt% of particles with a particle size of 5-3mm, and 20-40wt% of particles with a particle size of 3-1mm; the white corundum gradation meets the following requirements: 60-80wt% of particles with a particle size of 3-1mm, and 20-40wt% of fine powder with a particle size of 1-0.1mm; the silicon carbide gradation meets the following requirements: 60-75wt% of fine powder with a particle size of 100-200 meshes, and 25-40wt% of micro powder with a particle size of 200-400 meshes.
7. The blast furnace main ditch castable according to claim 1, characterized in that: In the dense corundum and white corundum, Al2O3≥99wt%, Fe2O3≤0.1wt%, SiO2≤0.1wt%; in the silicon carbide, SiC≥97wt%, SiO2≤0.4wt%, Fe2O3≤0.3wt%; The particle size D50 of the α-Al2O3 powder is 1 to 6 μm, and the Al2O3 in the α-Al2O3 powder is ≥ 99.0 wt%; The particle size D50 of the ρ-Al2O3 powder is 1 to 6 μm, and the Al2O3 in the ρ-Al2O3 powder is ≥ 98.0 wt%; The particle size D50 of the composite graphite particles is 15 to 60 μm; the particle size D50 of the graphite is 1 to 6 μm; the graphite is at least one of artificial graphite, natural graphite, and graphitized mesophase carbon microspheres; The particle size D50 of the aluminum nitride powder is 200-400 mesh; In the antioxidant, the particle size of magnesium carbide is 200-400 meshes, the particle size of boron carbide is 200-400 meshes, and the particle size of aluminum powder is 200-400 meshes.
8. The blast furnace main ditch castable according to claim 1, characterized in that: The anti-cracking fiber is made of organic fiber with a melting point of 90-160° C., a diameter of 4-8 μm, and a length of 8-15 mm; the water reducer is a polycarboxylate water reducer and / or sodium hexametaphosphate.
9. The method for preparing the main ditch castable for blast furnace iron tapping according to any one of claims 1 to 8, characterized in that: The following steps are involved: (S1) adding silicon carbide, α-Al2O3 powder, ρ-Al2O3 powder, composite graphite particles, aluminum nitride powder, and an antioxidant into a container and mixing and stirring to obtain a mixed fine material; (S2) adding dense corundum and white corundum into another container for mixing and stirring to obtain mixed granules; (S3) Under stirring, the mixed fine material obtained in (S1) is added to the mixed granular material obtained in (S2), and then explosion-proof fiber and water reducing agent are added for mixing and stirring to obtain a blast furnace iron tapping main ditch castable.
10. The method for pouring water into the main trough castable of a blast furnace as claimed in any one of claims 1 to 8, wherein the amount of water added is 2 to 3.5% of the total mass of the main trough castable.
Citation Information
Patent Citations
Al2O3-MA-SiC-C refractory castable material with carbon wrapped by nano Al2O3-SiC film and preparation method thereof
CN101767999A
Aluminum nitride refractory material and preparation method thereof
CN105461324A
Modified carbon source optimized Al2O3-SiC-C refractory castable for blast furnace iron tap channel as well as preparation method and application thereof
CN111620706A
Iron runner castable containing submicron composite antioxidant and preparation method of iron runner castable
CN115321996A
Fine powder composition for magnesia-graphite based castable, its production and magnesia-graphite based castable
JP1997110538A
Cited By
High-strength anti-cracking corrosion-resistant castable and preparation method thereof
CN122010540A
High-strength, crack-resistant and corrosion-resistant castable and preparation method thereof
CN122010540B