Double-active-site nickel monatomic catalyst as well as preparation method and application thereof in selective synthesis of furfuryl alcohol
By supporting nickel single atoms on nitrogen-doped porous carbon to form a dual-active site catalyst, the problems of high cost of precious metal catalysts and low conversion rate of non-precious metal catalysts are solved, and efficient and stable furfural selective hydrogen transfer reaction is achieved, reducing the Subsequent isolation and purification costs.
Patent Information
- Application Number
- CN202410875069.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing furfural catalytic transfer hydrogenation methods, noble metal catalysts are costly and have low selectivity, non-precious metal catalyst conversion rate is low, and the addition of Lewis base in the traditional method increases the subsequent reactant isolation and purification costs.
The high internal phase emulsion template method was used to synthesize nitrogen-doped porous carbon, and the nickel single atoms were loaded on the nitrogen-doped porous carbon by impregnation to form a dual-active site nickel single atom catalyst for catalyzing selective hydrogen transfer preparation of furfural Furfuryl alcohol avoids the use of Lewis base.
It achieves efficient, stable and economical catalytic performance, improves metal utilization, reduces preparation costs, and maintains high catalytic activity and selectivity. The furfural conversion rate and furfurfural alcohol yield both reach 99%, with good repeatability Utilization.
Smart Images

Figure CN118925768A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous solid catalysts, and particularly relates to a double-active-site nickel single-atom catalyst, a preparation method thereof, and application thereof in the selective synthesis of furfuryl alcohol. Background Art
[0002] Furfural is a platform molecule derived from lignocellulosic biomass. Its hydrogenation reaction can synthesize a variety of high value-added products, such as furfuryl alcohol and tetrahydrofuran furfural. Furfural is a typical α, β-unsaturated aldehyde with unsaturated C=C and C=O bonds. It is relatively active in chemical properties and is prone to oxidation, epoxidation and polymerization reactions. At present, there are two main methods for the selective hydrogenation of furfural to furfuryl alcohol: selective hydrogenation and catalytic transfer hydrogenation. Among them, the former uses H2 as a hydrogen donor, which not only has harsh reaction conditions, but also requires special facilities for transporting, storing and handling high-pressure H2. At the same time, high-pressure H2 is extremely easy to burn and explode when mixed with air. The above safety issues limit the application of this approach. Catalytic transfer hydrogenation uses cheap and readily available alcohols such as ethanol as hydrogen donors, which is simpler and safer in terms of experimental facilities and operations.
[0003] Among the reported catalysts for catalytic transfer hydrogenation of furfural, precious metal nanoparticle catalysts (Pt, Pd, Au, etc.) show high catalytic activity, but precious metal resources are limited and the production cost is high, and the selectivity for furfuryl alcohol is not high due to the strong adsorption of the active center to the C=C group. Non-precious metal nanoparticle catalysts (Ni, Fe, Co, etc.) have problems such as unsatisfactory conversion effect and low atomic utilization. Single atom catalysts (SACs) have become a hot topic in the field of catalysis because of their ultra-high metal atom utilization, excellent catalytic activity and selectivity. Patent Publication No. CN 117504897 A discloses a preparation method and application of a copper-palladium single-atom alloy catalyst with silica as a carrier, and the prepared atomic-level dispersed palladium-based catalyst shows excellent catalytic activity in the process of furfural hydrogenation reaction. Therefore, using SACs for the catalytic hydrogenation of furfural to prepare furfuryl alcohol can effectively improve the utilization of non-precious metals and greatly save costs.
[0004] Traditionally, according to the direct hydrogen transfer pathway of the CTH reaction, the SACs applied to the CTH of furfural rely on the adsorption of furfural and protonic alcohol (hydrogen donor) on transition metal atoms, which are Lewis acid sites. In order to strengthen the deprotonation of protonic alcohol, Lewis bases such as potassium tert-butoxide are usually added. However, the addition of Lewis bases greatly increases the cost of subsequent reactant separation and purification. In order to circumvent this problem, the present invention introduces pyridinic nitrogen as a Lewis basic site, and forms a dual active site SACs with Ni anchored on nitrogen-doped porous carbon, which is used for the catalytic transfer hydrogenation (CTH) reaction of furfural to furfuryl alcohol, wherein the Ni single atom site is combined with the hydroxyl group in the hydrogen donor and the carbonyl oxygen in the hydrogen acceptor as a Lewis acid site, and the adjacent non-coordinated pyridinic nitrogen is used as a Lewis basic site to attract the proton of the hydroxyl group in the hydrogen donor, showing a higher catalytic performance, avoiding the problem of separation and purification of subsequent products.
[0005] Porous carbon-based materials such as biochar, activated carbon and carbon nanotubes have become ideal carriers for SACs, which can effectively promote the transport of reactants and improve catalytic performance. In recent years, nitrogen-doped porous carbon materials have attracted extensive attention in the field of catalysis due to their stable structure and strong metal-support interaction. The pyridinic nitrogen in nitrogen-doped porous carbon can form a stable Ni-N bond with Ni atoms. x Coordination structure, prolonging the life of the catalyst; and electron transfer can occur, increasing the electron cloud density around the Ni atom, thereby improving the catalytic activity. Therefore, nitrogen-doped porous carbon materials with high pyridinic nitrogen content as carriers of metal single atoms will effectively improve the dispersibility and catalytic activity of metal single atoms on the carrier, thereby obtaining SACs with high catalytic activity and excellent stability. At the same time, studies have shown that the pore structure of the catalyst carrier will also greatly affect the substrate flux, mass transfer efficiency, and thus affect the overall catalytic activity. The high internal phase emulsion template method can qualitatively adjust the pore structure of the obtained porous material by adjusting the ratio of the internal and external phases. Therefore, the present invention adopts the high internal phase emulsion template method to prepare a carrier with high mass transfer efficiency, which synergizes with its dual active sites to greatly improve the catalytic activity.
[0006] At present, the preparation methods of SACs mainly include: coprecipitation method, impregnation method, atomic layer deposition method, sol-fixation method, and precipitation deposition method. Among them, the impregnation method is a method in which a solid powder or a formed solid (carrier or catalyst containing a host) is immersed in a solution containing a metal precursor, so that the metal precursor is adsorbed on the surface of the carrier, and then dried and calcined to form a uniformly dispersed single-atom metal carrier. This method is simple and easy to operate, does not require special equipment and complex procedures, and only requires the carrier material to be immersed in a catalyst precursor solution, so that the precursor ions can be fully adsorbed on the carrier surface to form a catalyst, which greatly reduces the preparation cost and difficulty. At the same time, during the preparation process, the catalyst precursor is completely adsorbed on the carrier surface, which can maximize the use of the catalyst precursor and avoid the waste of the precursor. The impregnation method can achieve precise control of the morphology, size and distribution of the catalyst particles by adjusting parameters such as the concentration of the catalyst precursor solution, the impregnation time and the temperature. Therefore, the catalyst prepared by the impregnation method has good morphology controllability and performance controllability. The impregnation method is simple to operate, mature in technology, easy to control parameters, high in metal utilization, and low in dosage. It is the most commonly used method for preparing traditional industrial catalysts. Therefore, the preparation of SACs by the impregnation method is extremely feasible. Summary of the invention
[0007] In view of the above problems, the present invention provides a dual-active site nickel single-atom catalyst, a preparation method thereof and an application in the selective synthesis of furfuryl alcohol. Nitrogen-doped porous carbon is synthesized by a high internal phase emulsion template method, and then nickel single atoms are loaded on the nitrogen-doped porous carbon by an impregnation method. After high-temperature calcination, a dual-active site nickel single-atom catalyst is obtained, and the catalyst is used to efficiently catalyze the selective hydrogen transfer of furfural to prepare furfuryl alcohol.
[0008] The present invention is achieved through the following technical solutions:
[0009] A dual-active-site nickel single-atom catalyst is disclosed. Nitrogen-doped porous carbon is synthesized by a high internal phase emulsion template method. Nickel single atoms are then loaded on the nitrogen-doped porous carbon by an impregnation method. After high-temperature calcination, a dual-active-site nickel single-atom catalyst is obtained.
[0010] Furthermore, the nickel metal content of the dual-active-site nickel single-atom catalyst is 0.26-0.27 wt % and the specific surface area is 60-65 cm 2 / g.
[0011] A method for preparing the double-active-site nickel single-atom catalyst as described above comprises the following steps:
[0012] (1) Raw material pretreatment: dissolving formaldehyde solution, resorcinol, melamine and urea in water at room temperature, stirring until the raw materials are completely dissolved, adjusting the pH value of the solution, and then homogenizing under heating conditions to obtain a prepolymer solution;
[0013] (2) Preparation of nitrogen-doped porous carbon: an emulsifier and HCl are sequentially added to a prepolymer solution, and then toluene is gradually added under stirring to form a stable water-in-oil emulsion, which is then stirred at a high speed, and then a polymerization reaction is carried out at a high temperature. The obtained porous polymer is ground into fine powder, and calcined at a high temperature under a nitrogen environment. After cooling, nitrogen-doped porous carbon is obtained;
[0014] (3) Preparation of the catalyst: Nitrogen-doped porous carbon and nickel nitrate hexahydrate are added to water and mixed. The resulting mixture is stirred at room temperature and then allowed to stand. The impregnated nitrogen-doped porous carbon is calcined at high temperature and cooled to obtain a dual-active site nickel single atom catalyst.
[0015] Furthermore, in step (1), the ratio of the formaldehyde solution, resorcinol, melamine and urea is 4-6 mL: 8-12 mmol: 4-6 mmol: 10 mmol; and the pH value of the solution is adjusted to 7.0-7.3 using anhydrous sodium carbonate.
[0016] Furthermore, in step (1), the heating temperature is 55 to 60° C., and the heating time is 15 to 20 minutes.
[0017] Furthermore, in step (2), the ratio of the prepolymer solution, the emulsifier, HCl and toluene is 30 mL: 4-5 g: 0.6-0.8 mL: 115-125 mL; the concentration of the emulsifier in the prepolymer solution is 8-10 wt %; and the emulsifier is Tween 20, Tween 80 or sodium dodecyl sulfate.
[0018] Furthermore, in step (2), the polymerization reaction is performed at a temperature of 80-90°C for 22-24 hours; the high-temperature calcination is performed at a rate of 3-5°C / min to 800-1000°C for 1.5-2 hours; and the high-speed stirring is performed at a rotation speed of 900-1100 r / min for 3-5 minutes.
[0019] Furthermore, in step (3), the mass ratio of the nitrogen-doped porous carbon to nickel nitrate hexahydrate is 1:0.002-0.003.
[0020] Furthermore, in step (3), the high temperature calcination is carried out at a rate of 3 to 5°C / min and the temperature is raised to 400 to 500°C for 1.5 to 2 hours; the stirring time is 18 to 20 hours; and the standing time is 3 to 4 hours.
[0021] An application of the double-active-site nickel single-atom catalyst as described above in catalyzing the selective hydrogen transfer of furfural to prepare furfuryl alcohol.
[0022] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0023] 1. The present invention adopts a high internal phase emulsion template method to synthesize nitrogen-doped porous carbon, and then loads Ni single atoms on the nitrogen-doped porous carbon by an impregnation method. After high-temperature calcination, a dual-active-site nickel single-atom catalyst is obtained, which is used to efficiently catalyze furfural and selectively catalyze hydrogen transfer to furfuryl alcohol. The present invention successfully constructs a green, economical, stable-performance, and directional catalytic Ni single-atom catalyst with dual active sites by combining an impregnation method with a high-temperature calcination strategy, providing a new method strategy for the design and development of functional catalysts, effectively promoting the high-value utilization of furfural, and has important research significance.
[0024] 2. Nitrogen-doped porous carbon-based materials have high electrical conductivity and mechanical strength. The present invention uses an impregnation method to evenly disperse Ni atoms on the nitrogen-doped porous carbon material to form a highly dispersed catalyst. The Ni-N bond formed by Ni atoms and pyridine nitrogen in the nitrogen-doped porous carbon carrier x The structure increases the migration and diffusion of carriers between N and Ni, and enhances the electron cloud density near the Ni atom. Due to the synergistic effect of Ni and pyridinic nitrogen, it is beneficial to stably load the active component Ni single atom on the nitrogen-doped porous carbon support to construct a supported catalyst with strong metal-support interaction.
[0025] 3. The present invention uses nitrogen-doped porous carbon as a precursor and adopts an impregnation method to load Ni single atoms on the nitrogen-doped porous carbon. The high content of pyridinic nitrogen in the nitrogen-doped porous carbon can effectively promote the uniform dispersion and stability of Ni metal in the nitrogen-doped porous carbon, which is beneficial to the formation of a strong interaction between Ni metal and nitrogen-doped porous carbon after calcination. The obtained Ni single atom catalyst has a stable structure and good reusability, thereby improving the efficiency and economic feasibility of the catalyst in practical applications.
[0026] 4. The present invention effectively improves the dispersibility of metal-based components by loading metals through the impregnation method; a large amount of pyridinic nitrogen in the nitrogen-doped porous carbon carrier is used to anchor Ni atoms, successfully constructing a stable metal-carrier structure; the Ni-N bond formed by Ni atoms and pyridinic nitrogen in the carrier x structure, changing the electron cloud density between them and giving Ni single atoms a stronger bonding effect. After high-temperature calcination, they can be stably immobilized on the carrier, which makes the catalyst able to be recycled many times and has good reusability.
[0027] 5. The preparation method of the catalyst of the present invention is simple to operate, the raw materials are easily available, the conditions are simple and mild, and the production cost is low. The catalyst of the present invention has a good catalytic conversion efficiency for furfural. When the catalyst is used in the process of catalyzing furfural to prepare furfuryl alcohol, the conversion rate of furfural and the activity of furfuryl alcohol are high, the conversion rate of furfural can reach 99%, and the yield of furfuryl alcohol can reach 99%. At the same time, after the catalyst of the present invention is used 5 times, the conversion rate of furfural is still 99%, and the selectivity of the target product furfuryl alcohol is also maintained at more than 98%, which has a good application prospect for the efficient conversion of furfural to prepare furfuryl alcohol. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Ni1 / NC prepared in Example 1 and Comparative Examples 1-4 900 、Ni NPs / NC 900 、Ni1 / NC 800 、Ni1 / NC 1000 and NC 900 XRD pattern of .
[0029] Figure 2 Ni1 / NC prepared in Example 1 900 SEM image of .
[0030] Figure 3 Ni1 / NC prepared in Example 1 900 TEM image of.
[0031] Figure 4 Ni prepared in Comparative Example 1 NPs / NC 900 TEM image of.
[0032] Figure 5 Ni1 / NC prepared in Example 1 900 EDX image.
[0033] Figure 6 Ni1 / NC prepared in Example 1 900 AC-HAADF-STEM image.
[0034] Figure 7 Ni1 / NC prepared in Example 1 900 XPS graph.
[0035] Figure 8 Ni1 / NC prepared in Example 1 900 N2 adsorption-desorption isotherm diagram. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below by way of examples. These examples are only used to illustrate the present invention and do not limit the protection scope of the present invention.
[0037] Example 1
[0038] Preparation of double active site nickel single atom catalysts:
[0039] (1) Raw material pretreatment: 5 mL of formaldehyde solution, 10 mmol of resorcinol, 5 mmol of melamine and 10 mmol of urea were dissolved in 23 mL of deionized water at room temperature, and the mixture was stirred until all the raw materials were completely dissolved. Subsequently, the pH value of the solution was accurately adjusted to 7.1 using anhydrous sodium carbonate. The mixture was then placed in a water bath maintained at 60°C, the homogenized mixture was stirred at a speed of 300 r / min, and heated for 20 min to obtain a prepolymer solution;
[0040] (2) Preparation of nitrogen-doped porous carbon: 4 g of emulsifier Tween 20 was added to 30 mL of prepolymer solution until its concentration reached 10 wt %. Subsequently, 0.7 mL of 1 mol / L HCl was added to the prepolymer solution to catalyze the subsequent reaction. Then, 120 mL of toluene as the oil phase was gradually added to the water phase at a stirring speed of 500 r / min to form a stable water-in-oil emulsion. Subsequently, high-speed stirring was performed at a speed of 1000 r / min for 3 minutes to ensure its uniformity. The uniform water-in-oil emulsion was then polymerized at a temperature of 85°C for 24 hours. After the reaction was completed, the completely dried porous polymer was ground into fine powder using a mortar and pestle. The prepared porous polymer powder was then calcined in a nitrogen environment at a temperature increase rate of 3°C / min to a final temperature of 900°C, which was maintained at this temperature for 2 hours. After cooling, nitrogen-doped porous carbon (denoted as NC) was obtained. 900 );
[0041] (3) Preparation of catalyst: 1.00 g of nitrogen-doped porous carbon and 0.0025 g of nickel nitrate hexahydrate were added to 10 mL of deionized water, and the mixture was stirred at 300 r / min for 20 h at room temperature using the initial wet impregnation method, and then allowed to stand for 4 h. The impregnated nitrogen-doped porous carbon was calcined at 400 °C with a heating rate of 3 °C / min for 2 h. After cooling, a dual-active-site nickel single-atom catalyst (denoted as Ni1 / NC 900 ).
[0042] Example 2
[0043] Preparation of double active site nickel single atom catalysts:
[0044] (1) Raw material pretreatment: 4 mL of formaldehyde solution, 8 mmol of resorcinol, 5 mmol of melamine and 10 mmol of urea were dissolved in 23 mL of deionized water at room temperature, and the mixture was stirred until all the raw materials were completely dissolved. Subsequently, the pH value of the solution was accurately adjusted to 7.2 using anhydrous sodium carbonate. The mixture was then placed in a water bath maintained at 55°C, the homogenized mixture was stirred at a speed of 300 r / min, and heated for 20 min to obtain a prepolymer solution;
[0045] (2) Preparation of nitrogen-doped porous carbon: 4.1 g of emulsifier Tween 20 was added to 30 mL of prepolymer solution until its concentration reached 8 wt %. Subsequently, 0.6 mL of 1 mol / L HCl was added to the prepolymer solution to catalyze the subsequent reaction. Then, 125 mL of toluene as the oil phase was gradually added to the water phase at a stirring speed of 500 r / min to form a stable water-in-oil emulsion. Subsequently, high-speed stirring was performed at a speed of 900 r / min for 5 minutes to ensure its uniformity. The uniform water-in-oil emulsion was then polymerized at a temperature of 80°C for 24 hours. After the reaction was completed, the completely dried porous polymer was ground into fine powder using a mortar and pestle. The prepared porous polymer powder was then calcined in a nitrogen environment at a temperature increase rate of 5°C / min to a final temperature of 870°C, which was maintained for 2 hours. After cooling, nitrogen-doped porous carbon was obtained;
[0046] (3) Preparation of catalyst: 1.00 g of nitrogen-doped porous carbon and 0.0025 g of nickel nitrate hexahydrate were added to 10 mL of deionized water, and the mixture was stirred at 300 r / min for 18 h at room temperature using the initial wet impregnation method, and then allowed to stand for 3 h. The impregnated nitrogen-doped porous carbon was calcined at 400 °C with a heating rate of 3 °C / min for 2 h. After cooling, a dual-active-site nickel single-atom catalyst was obtained.
[0047] Example 3
[0048] Preparation of double active site nickel single atom catalysts:
[0049] (1) Raw material pretreatment: 5 mL of formaldehyde solution, 12 mmol of resorcinol, 6 mmol of melamine and 10 mmol of urea were dissolved in 23 mL of deionized water at room temperature, and the mixture was stirred until all the raw materials were completely dissolved. Subsequently, the pH value of the solution was accurately adjusted to 7.3 using anhydrous sodium carbonate. The mixture was then placed in a water bath maintained at 60°C, the homogenized mixture was stirred at a speed of 300 r / min, and heated for 15 min to obtain a prepolymer solution;
[0050] (2) Preparation of nitrogen-doped porous carbon: 4.3 g of emulsifier Tween 80 was added to 30 mL of prepolymer solution until its concentration reached 9 wt %. Subsequently, 0.8 mL of 1 mol / L HCl was added to the prepolymer solution to catalyze the subsequent reaction. Then, 125 mL of toluene as the oil phase was gradually added to the water phase at a stirring speed of 500 r / min to form a stable water-in-oil emulsion. Subsequently, high-speed stirring was performed at a speed of 1000 r / min for 4 minutes to ensure its uniformity. The uniform water-in-oil emulsion was then polymerized at a temperature of 90°C for 22 hours. After the reaction was completed, the completely dried porous polymer was ground into fine powder using a mortar and pestle. The prepared porous polymer powder was then calcined in a nitrogen environment at a temperature increase rate of 3°C / min to a final temperature of 930°C, which was maintained at this temperature for 1.5 hours. After cooling, nitrogen-doped porous carbon was obtained;
[0051] (3) Preparation of catalyst: 1.00 g of nitrogen-doped porous carbon and 0.002 g of nickel nitrate hexahydrate were added to 10 mL of deionized water, and the mixture was stirred at 300 r / min for 20 h at room temperature using the initial wet impregnation method, and then allowed to stand for 4 h. The impregnated nitrogen-doped porous carbon was calcined at 400 °C, with a heating rate of 5 °C / min, and the calcination process lasted for 1.5 h. After cooling, a dual-active site nickel single atom catalyst was obtained.
[0052] Example 4
[0053] Preparation of double active site nickel single atom catalysts:
[0054] (1) Raw material pretreatment: 6 mL of formaldehyde solution, 10 mmol of resorcinol, 4 mmol of melamine and 10 mmol of urea were dissolved in 23 mL of deionized water at room temperature, and the mixture was stirred until all the raw materials were completely dissolved. Subsequently, the pH value of the solution was accurately adjusted to 7.1 using anhydrous sodium carbonate. The mixture was then placed in a water bath maintained at 60°C, the homogenized mixture was stirred at a speed of 300 r / min, and heated for 20 min to obtain a prepolymer solution;
[0055] (2) Preparation of nitrogen-doped porous carbon: 4.9 g of emulsifier sodium dodecyl sulfate was added to 30 mL of prepolymer solution until its concentration reached 10 wt%. Subsequently, 0.8 mL of 1 mol / L HCl was added to the prepolymer solution to catalyze the subsequent reaction. Then, 123 mL of toluene as the oil phase was gradually added to the water phase at a stirring speed of 500 r / min to form a stable water-in-oil emulsion. Subsequently, high-speed stirring was performed at a speed of 1100 r / min for 3 minutes to ensure its uniformity. The uniform water-in-oil emulsion was then polymerized at a temperature of 85°C for 24 hours. After the reaction was completed, the completely dried porous polymer was ground into fine powder using a mortar and pestle. The prepared porous polymer powder was then calcined in a nitrogen environment at a temperature increase rate of 5°C / min to a final temperature of 920°C, which was maintained at this temperature for 21.5 hours. After cooling, nitrogen-doped porous carbon was obtained;
[0056] (3) Preparation of catalyst: 1.00 g of nitrogen-doped porous carbon and 0.003 g of nickel nitrate hexahydrate were added to 10 mL of deionized water, and the mixture was stirred at 300 r / min for 20 h at room temperature using the initial wet impregnation method, and then allowed to stand for 4 h. The impregnated nitrogen-doped porous carbon was calcined at 500 °C with a heating rate of 5 °C / min for 2 h. After cooling, a dual-active-site nickel single-atom catalyst was obtained.
[0057] Comparative Example 1
[0058] The difference between Comparative Example 1 and Example 1 is that the amount of nickel nitrate hexahydrate used in Comparative Example 1 is 0.005 g, and the other preparation conditions are the same as those in Example 1, and a dual-active site nickel nanoparticle catalyst (denoted as Ni NPs / NC 900 ).
[0059] Comparative Example 2
[0060] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, when preparing nitrogen-doped porous carbon, the final calcination temperature is 800°C, and the other preparation conditions are the same as those in Example 1, and a double-active-site nickel single-atom catalyst (denoted as Ni1 / NC 800 ).
[0061] Comparative Example 3
[0062] The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, when preparing nitrogen-doped porous carbon, the final calcination temperature is 1000°C, and the other preparation conditions are the same as those in Example 1, and a double-active-site nickel single-atom catalyst (denoted as Ni1 / NC 1000 ).
[0063] Comparative Example 4
[0064] The difference between Comparative Example 4 and Example 1 is that in Comparative Example 4, only nitrogen-doped porous carbon is prepared without nickel metal impregnation treatment (denoted as NC 900 ).
[0065] Material Characterization Analysis
[0066] (I) XRD analysis
[0067] The Ni1 / NC prepared in Example 1 and Comparative Examples 1-4 were analyzed by X-ray diffractometer (XRD). 900 、Ni NPs / NC 900 、Ni1 / NC 800 、Ni1 / NC 1000 and NC 900 Characterization analysis was performed, and the characterization results were as follows Figure 1 As shown. Figure 1 It can be seen that Ni1 / NC 900 The samples have amorphous carbon peaks at 23.7° and 44.1°, respectively, which indicates that Ni1 / NC 900 There is no obvious nickel metal aggregation in the catalyst, that is, no nickel nanoparticles are present. NPs / NC 900 In the experiment, the peaks of Ni metal were found at 31.6° and 45.3°, which were analyzed to be NiO x diffraction peaks, which confirms that Ni NPs / NC 900 The presence of Ni metal nanoparticles.
[0068] (ii) SEM analysis
[0069] The Ni1 / NC prepared in Example 1 was examined by scanning electron microscopy (SEM). 900 The characterization results are as follows: Figure 2 As shown. Figure 2 Amorphous carbon can be observed in the SEM image, and Ni1 / NC 900 There are a large number of mesopores with uniform pore size distribution on the surface of the carrier, which proves the successful preparation of the carrier with high mass transfer efficiency.
[0070] (III) TEM analysis
[0071] The Ni1 / NC prepared in Example 1 and Comparative Example 1 were examined by transmission electron microscopy (TEM). 900 and Ni NPs / NC 900 Characterization analysis was performed, and the characterization results were as follows Figure 3 and 4 shown. Figure 3 (a) and Figure 3 (b) represents Ni1 / NC 900 TEM images of the catalyst at different scales. Figure 3 (a) It can be observed that Ni1 / NC 900 The amorphous carbon measured in the above equation is 0.04, and no Ni metal aggregation is observed. Figure 4 It can be seen that Ni NPs / NC 900 Multiple Ni metals aggregated into nanoclusters in the catalyst, with lattice fringes of 0.28 nm, suspected to be NiO x , indicating that excessive Ni metal content leads to metal aggregation. NPs / NC 900 The catalytic effect is far inferior to Ni1 / NC 900 Good reasons.
[0072] (IV) EDX analysis
[0073] The Ni1 / NC prepared in Example 1 was analyzed by energy dispersive X-ray spectrometry (EDX). 900 The characterization results are as follows: Figure 5 As shown. Figure 5 (ae) It can be seen that Ni1 / NC 900 The catalyst contains four elements: C, N, O, and Ni, proving that Ni was successfully loaded onto the carrier. Moreover, the Ni element was evenly dispersed, and no Ni nanoparticles were observed.
[0074] (V) AC HAADF-STEM analysis
[0075] The Ni1 / NC prepared in Example 1 was imaged using a spherical aberration corrected high angle annular dark field scanning transmission microscope (AC HAADF-STEM). 900 The characterization results are as follows: Figure 6 As shown. Figure 6 It can be seen that Ni1 / NC 900 The single atomic points marked by yellow circles are clearly shown, showing that the Ni single atoms are isolated and evenly dispersed in the NC 900 This is consistent with the EDX characterization results.
[0076] (VI) XPS analysis
[0077] The Ni1 / NC prepared in Example 1 was analyzed by X-ray photoelectron spectroscopy (XPS). 900 The surface chemical state and elemental composition of Figure 7 As shown. Figure 7(a) It can be seen that there are three fitting peaks in the XPS spectrum of C1s in the catalyst, the peak corresponding to C=N is shown at 285.8eV, and there are two classic peaks related to CC / C=C and C=O. Figure 7 (b) It can be seen that the XPS spectrum of N1s in the catalyst shows peaks of pyridine-N (398.8 eV), Ni-N (399.1 eV), pyrrole-N (399.7 eV), graphite-N (410.0 eV) and oxide-N (403.4 eV), while the peak of metallic nitrogen (397.0 eV) does not exist, which further confirms that there are no nickel nanoparticles in the catalyst. In addition, part of the nitrogen in the pyridine-N form coordinates with nickel to form Ni-N (399.1 eV), and electron transfer occurs at Ni-N x In the coordination of Ni1 / NC, the electrons are transferred from N to Ni, thereby increasing the electron cloud density at the center of the Ni atom and improving its catalytic activity. 900 In the Ni 2p XPS spectrum, the peaks at 854.1 and 872.6 eV correspond to the Ni 2p 3 / 2 and Ni 2p 1 / 2 , which proves that 2+ existence.
[0078] (VII) ICP-OES analysis
[0079] The Ni1 / NC prepared in Example 1 was analyzed by inductively coupled plasma optical emission spectrometry (ICP-OES). 900 The characterization analysis showed that Ni1 / NC 900 The nickel metal content in the catalyst is 0.27 wt%.
[0080] (VIII) Specific surface area analysis
[0081] The Ni1 / NC prepared in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were subjected to N2 adsorption-desorption. 900 、Ni NPs / NC 900 、Ni1 / NC 800 、Ni1 / NC 1000 The characterization results are as follows: Figure 8 As shown. Figure 8 It can be seen that Ni1 / NC 900 The specific surface area of the catalyst is 62.4 cm 2 / g, the mesopores formed make the catalytic effect better and can effectively improve the efficiency of the catalytic reaction. NPs / NC 900 The specific surface area is only 19.0 cm 2 / g, which may be due to the presence of Ni nanoparticles, making Ni NPs / NC 900 The pores of the catalyst are blocked. And Ni1 / NC 800 and Ni1 / NC 1000 The specific surface areas are 89.4 cm 2 / g and 48.1cm 2 / g. This is because in Ni1 / NC 1000 During the preparation process, the pyrolysis temperature is too high, which will lead to excessive decomposition of the porous polymer powder, resulting in pore collapse and the formation of more macropores. 800 If the pyrolysis temperature of Ni1 / NC is too low, the porous polymer powder will not be fully decomposed, forming more micropores. 1000 The macropores formed and Ni1 / NC 800 The formed micropores are not as good as Ni1 / NC in catalytic effect 900 of mesopores.
[0082] Application Example 1
[0083] Take the Ni1 / NC prepared in Example 1 900 Catalyst, 2mmol furfural, 5mL isopropanol and 15mg catalyst are placed in a hydrothermal reactor of a high-pressure reactor, and then the reactor is placed in an oil bath at 80°C. After reacting for 60 minutes, the reactor is taken out of the oil bath and quickly cooled in a water bath to stop the reaction. The obtained reaction solution is cooled and then filtered through a filter membrane with a pore size of 0.22μm to obtain furfuryl alcohol. It is determined that the conversion rate of furfural is 88% and the selectivity of furfuryl alcohol is 99%.
[0084] Application Example 2
[0085] The difference between Application Example 2 and Application Example 1 is that the oil bath temperature in Application Example 2 is 90° C., and the other preparation conditions are the same as those in Application Example 1. It was determined that the conversion rate of furfural was 96%, and the selectivity of furfuryl alcohol was 99%.
[0086] Application Example 3
[0087] The difference between Application Example 3 and Application Example 1 is that the oil bath temperature in Application Example 3 is 100° C., and the other preparation conditions are the same as those in Application Example 1. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 99%.
[0088] Application Example 4
[0089] The difference between Application Example 4 and Application Example 1 is that the oil bath temperature in Application Example 4 is 110° C., and the other preparation conditions are the same as those in Application Example 1. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 82%.
[0090] Application Example 5
[0091] The difference between Application Example 5 and Application Example 1 is that the oil bath temperature in Application Example 5 is 120° C., and the other preparation conditions are the same as those in Application Example 1. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 80%.
[0092] Application Example 6
[0093] The difference between Application Example 6 and Application Example 3 is that the reaction time in Application Example 6 is 20 min, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 46%, and the selectivity of furfuryl alcohol was 99%.
[0094] Application Example 7
[0095] The difference between Application Example 7 and Application Example 3 is that the reaction time in Application Example 7 is 40 min, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 83%, and the selectivity of furfuryl alcohol was 99%.
[0096] Application Example 8
[0097] The difference between Application Example 8 and Application Example 3 is that the reaction time in Application Example 8 is 80 min, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 86%.
[0098] Application Example 9
[0099] The difference between Application Example 9 and Application Example 3 is that the reaction time in Application Example 9 is 100 min, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 84%.
[0100] Application Example 10
[0101] The difference between Application Example 10 and Application Example 3 is that the amount of catalyst used in Application Example 10 is 5 mg, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 42%, and the selectivity of furfuryl alcohol was 99%.
[0102] Application Example 11
[0103] The difference between Application Example 11 and Application Example 3 is that the amount of catalyst used in Application Example 11 is 10 mg, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 86%, and the selectivity of furfuryl alcohol was 99%.
[0104] Application Example 12
[0105] The difference between Application Example 12 and Application Example 3 is that the amount of catalyst used in Application Example 12 is 20 mg, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 99%.
[0106] Application Example 13
[0107] The difference between Application Example 13 and Application Example 3 is that the amount of catalyst used in Application Example 13 is 25 mg, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 99%.
[0108] Application Example 14
[0109] The difference between Application Example 14 and Application Example 3 is that the amount of isopropanol used in Application Example 14 is 3 mL, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 64%, and the selectivity of furfuryl alcohol was 95%.
[0110] Application Example 15
[0111] The difference between Application Example 15 and Application Example 3 is that the amount of isopropanol used in Application Example 15 is 4 mL, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 87%, and the selectivity of furfuryl alcohol was 97%.
[0112] Application Example 16
[0113] The difference between Application Example 16 and Application Example 3 is that the amount of isopropanol used in Application Example 16 is 6 mL, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 99%.
[0114] Application Example 17
[0115] The difference between Application Example 17 and Application Example 3 is that the amount of isopropanol used in Application Example 17 is 7 mL, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 99%.
[0116] Application Example 18
[0117] The difference between Application Example 18 and Application Example 3 is that the catalyst in Application Example 18 is the catalyst used five times in Application Example 3, and the other preparation conditions are the same as those in Application Example 3. It was determined that the conversion rate of furfural was 99%, and the selectivity of furfuryl alcohol was 98%.
[0118] Application Comparative Example 1
[0119] The difference between the comparative example 1 and the example 3 is that the catalyst in the comparative example 1 is Ni prepared in the comparative example 1. NPs / NC 900 The catalyst and other preparation conditions were the same as those in Application Example 3. It was determined that the conversion rate of furfural was 87% and the selectivity of furfuryl alcohol was 87%.
[0120] Application Comparative Example 2
[0121] The difference between Application Example 2 and Application Example 3 is that the catalyst in Application Example 2 is Ni1 / NC prepared in Application Example 2. 800 The catalyst and other preparation conditions were the same as those in Application Example 3. It was determined that the conversion rate of furfural was 84% and the selectivity of furfuryl alcohol was 87%.
[0122] Application Comparative Example 3
[0123] The difference between the comparative example 3 and the example 3 is that the catalyst in the comparative example 3 is Ni1 / NC prepared in the comparative example 3. 1000 The catalyst and other preparation conditions were the same as those in Application Example 3. It was determined that the conversion rate of furfural was 83% and the selectivity of furfuryl alcohol was 86%.
[0124] Application Comparative Example 4
[0125] The difference between the comparative example 4 and the example 3 is that the catalyst in the comparative example 4 is NC prepared in the comparative example 4. 900 The catalyst and other preparation conditions were the same as those in Application Example 3. It was determined that the conversion rate of furfural was 5% and the selectivity of furfuryl alcohol was 0%.
[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A double active site nickel single atom catalyst, characterized in that: Nitrogen-doped porous carbon was synthesized by high internal phase emulsion template method, and then nickel single atoms were loaded on the nitrogen-doped porous carbon by impregnation method. After high-temperature calcination, a dual-active site nickel single atom catalyst was obtained.
2. The double active site nickel single atom catalyst according to claim 1, characterized in that: The nickel metal content of the double active site nickel single atom catalyst is 0.26-0.27 wt % and the specific surface area is 60-65 cm 2 / g.
3. A method for preparing a dual-active-site nickel single-atom catalyst as claimed in claim 1 or 2, characterized in that: The following steps are involved: (1) Raw material pretreatment: dissolving formaldehyde solution, resorcinol, melamine and urea in water at room temperature, stirring until the raw materials are completely dissolved, adjusting the pH value of the solution, and then homogenizing under heating conditions to obtain a prepolymer solution; (2) Preparation of nitrogen-doped porous carbon: an emulsifier and HCl are sequentially added to a prepolymer solution, and then toluene is gradually added under stirring to form a stable water-in-oil emulsion, which is then stirred at a high speed, and then a polymerization reaction is carried out at a high temperature. The obtained porous polymer is ground into fine powder, and calcined at a high temperature under a nitrogen environment. After cooling, nitrogen-doped porous carbon is obtained; (3) Preparation of the catalyst: Nitrogen-doped porous carbon and nickel nitrate hexahydrate are added to water and mixed. The resulting mixture is stirred at room temperature and then allowed to stand. The impregnated nitrogen-doped porous carbon is calcined at high temperature and cooled to obtain a dual-active site nickel single atom catalyst.
4. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (1), the ratio of the formaldehyde solution, resorcinol, melamine and urea is 4-6 mL: 8-12 mmol: 4-6 mmol: 10 mmol; and the pH value of the solution is adjusted to 7.0-7.3 using anhydrous sodium carbonate.
5. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (1), the heating temperature is 55-60° C. and the heating time is 15-20 min.
6. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (2), the ratio of the prepolymer solution, emulsifier, HCl and toluene is 30mL:4-5g:0.6-0.8mL:115-125mL; the concentration of the emulsifier in the prepolymer solution is 8-10wt%; the emulsifier is Tween 20, Tween 80 or sodium dodecyl sulfate.
7. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (2), the polymerization reaction is carried out at a temperature of 80-90°C for 22-24 hours; the high-temperature calcination is carried out at a rate of 3-5°C / min to 800-1000°C for 1.5-2 hours; and the high-speed stirring is carried out at a rotation speed of 900-1100 r / min for 3-5 minutes.
8. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (3), the mass ratio of the nitrogen-doped porous carbon to nickel nitrate hexahydrate is 1:0.002-0.
003.
9. The method for preparing a double-active-site nickel single-atom catalyst according to claim 3, characterized in that: In step (3), the high temperature calcination is carried out at a rate of 3 to 5°C / min and the temperature is raised to 400 to 500°C for 1.5 to 2 hours; the stirring time is 18 to 20 hours; and the standing time is 3 to 4 hours.
10. Use of the dual-active-site nickel single-atom catalyst as claimed in claim 1 or 2 in catalyzing the selective hydrogenation of furfural to prepare furfuryl alcohol.
Citation Information
Cited By
A highly dispersed nickel-based carbon-nitrogen catalyst, preparation method and application thereof