Through the online thermal replenishment method, the thermal feed of magnesium oxide and other materials is used to quickly sinter and repair it after the ladle is turned over and slag is over, which solves the problems of inconvenient operation and high equipment requirements of the existing ladle lining maintenance methods, and achieves low cost. Efficient ladle repair extends ladle life and improves the working environment.

CN118926518APending Publication Date: 2024-11-12SHANDONG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101126.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing ladle lining maintenance methods have problems such as inconvenient operation, high equipment demand, large consumption of refractory materials, and affected production rhythm, especially in high-temperature environments, which are difficult to achieve rapid and low-cost repair.

Method used

The online thermal repair method is adopted to apply thermal feed to the slag groove after the ladle is turned over and over, and the thermal feed consisting of magnesium oxide, alumina, carbon and binding agent is used to perform rapid sintering and repair, avoiding additional equipment and dust. question.

Benefits of technology

It realizes rapid repair of the ladle slag trench parts, simplifies operations, reduces equipment costs and energy consumption, extends the ladle life, and improves the working environment for workers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of steel and iron smelting, in particular to a steel ladle online hot patching method which comprises the following steps: S1, determining a steel ladle to be repaired and a repair heat according to the slag runner depth of the steel ladle; s2, a steel ladle is laid flat after being turned over and subjected to slag pouring, and a hot patching material is put into a slag runner; and S3, in the steel ladle in which the hot patching material is put, the slag is ensured to be viscous during the next furnace refining. According to the online hot patching method for the steel ladle, the ladle lining at the slag runner part of the steel ladle can be quickly repaired, and emergency repair can also be carried out; the operation is simple and convenient, and large equipment cost investment is not needed; a moulding bed does not need to be supported; rapid sintering can be achieved, and energy is saved; dust is not generated when hot patching materials are fed, the labor environment of workers is improved, time and labor are saved, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, in particular to an online hot patching method for a ladle. Background Art

[0002] As the main container for molten steel from converters or electric furnaces, the ladle is responsible for transporting the molten steel to the refining process for reprocessing or continuous casting for pouring. With the development of steelmaking technology, especially the increase in continuous casting ratio and the development of refining technology outside the furnace: the tapping temperature is increased, the retention time of molten steel in the ladle is prolonged, and the molten steel in the ladle needs to be deoxidized, degassed and the chemical composition adjusted, which aggravates the erosion of slag on the refractory material of the ladle lining, reduces the life of the ladle lining and increases safety hazards. The consumption of refractory materials for ladles increases, the number of ladles put into use increases, and the consumption of energy such as coal gas increases, resulting in higher steelmaking costs. Therefore, seeking new ways to increase the service life of ladles is an important issue for many steel companies.

[0003] During the use, the ladle lining gradually becomes thinner due to factors such as erosion, penetration and slag invasion by molten steel. This is mainly caused by the peeling caused by the expansion of cracks parallel to the hot surface, and the melting loss caused by the penetration of molten steel and slag. During the entire process of ladle transportation, the refractory materials are corroded and penetrated by molten steel and slag, resulting in the damage of the refractory materials of the ladle lining. Generally, the damage to the steel surface (i.e., slag pouring surface) and the slag line is the most serious.

[0004] The commonly used maintenance methods for ladle linings currently include cold repair, unpacking and re-casting after one-time use, or hot spraying. Among them, cold repair has many inconveniences in terms of process and economy. First, after the ladle is cooled and the residue is cleaned, the mold is placed in the old lining, and the castable with good fluidity is poured into the gap for vibration molding. After that, it must go through the processes of curing, demoulding, baking, etc. before it can be put into use. The work intensity of cold repair and residue cleaning is high, and there is a lot of dust on site. It needs to be used in conjunction with dust removal equipment, and strict requirements are placed on the fluidity of the castable. Unpacking and re-casting after one-time use consumes a lot of refractory materials, which increases the cost of steelmaking. Hot spraying requires the use of corresponding spraying equipment, and there are certain requirements for the spraying material, such as the particle size and high-temperature anti-explosion performance of the spraying material. Due to the participation of water, the baking and sintering time needs to be extended, which in turn affects the production rhythm.

[0005] Therefore, there is an urgent need for an easy-to-operate ladle repair method that can reduce the required equipment and improve the repair efficiency while ensuring the ladle performance. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and to provide a method for online hot patching of a ladle, which can complete the online hot patching of the ladle lining in a relatively short time without the need for additional equipment.

[0007] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0008] A method for online hot patching of a ladle comprises the following steps:

[0009] S1. Determine the ladle to be repaired and the repair heat according to the slag groove depth of the ladle;

[0010] S2. After the ladle is turned over and the slag is emptied, it is laid flat and hot patching material is added into the slag groove;

[0011] S3. After the hot patch material is put into the ladle, ensure that the slag is viscous during the next refining.

[0012] Preferably, in step S1,

[0013] When the depth of the ladle slag groove is less than 60mm, repair should be postponed for one or two furnaces;

[0014] When the depth of the ladle slag groove is between 60mm and 100mm, repairs should be carried out immediately for the next batch after the operation of the current batch is completed.

[0015] Preferably, in step S2, when the ladle is slag-drained, the ladle is tilted and left to stand for 1 min without slag flowing out, which means that the slag in the ladle is completely drained, and subsequent heat addition and feeding operations are performed.

[0016] Preferably, in step S2, the hot patch material consists of magnesium oxide, aluminum oxide, carbon, a binder and water, wherein magnesium oxide accounts for ≥76wt% of the total mass of the hot patch material, carbon accounts for ≥14wt% of the total mass of the hot patch material, aluminum oxide accounts for ≥5wt% of the total mass of the hot patch material, the binder accounts for ≥3wt% of the total mass of the hot patch material, the moisture content of the hot patch material is ≤1.0wt%, and the particle size of the hot patch material is 1mm-5mm; further preferably, the binder consists of equal amounts of modified asphalt and phenolic resin.

[0017] Preferably, in step S2, hot patching material is added to make the slag groove flush with the slag line bricks adjacent to the slag groove in the ladle; further preferably, the hot patching material is added in batches, and the amount added in each batch is 5±1 kg.

[0018] Beneficial effects:

[0019] The method for online hot patching of a ladle provided by the present invention can quickly patch the lining of the slag groove of the ladle, and can also perform emergency patching; the operation is simple and convenient, and does not require a large investment in equipment costs; no supporting mold is required; rapid sintering is possible, saving energy; no dust is generated when hot patching materials are added, thus improving the working environment of workers, saving time, labor, and cost. DETAILED DESCRIPTION

[0020] The present invention will be further described below with reference to specific embodiments, but is not limited thereto.

[0021] Example 1

[0022] A ladle online hot patching method,

[0023] In this embodiment, the age of online ladle 7# is 17 times, and grooves are eroded at the slag line of the slag pouring surface. The depth of the slag grooves is measured to be 40 mm, so the repair of two furnaces is delayed. The time for replacing the water nozzle is selected at the 19th time, and the slag grooves on the slag pouring surface are quickly hot-patched.

[0024] In this embodiment, magnesium oxide accounts for 76.22wt% of the total mass of the hot patch material, C accounts for 14.16wt% of the total mass of the hot patch material, aluminum oxide accounts for 5.41wt% of the total mass of the hot patch material, adhesive accounts for 3.151wt% of the total mass of the hot patch material, and the moisture content is 0.70wt%. After the 19th furnace is poured, a crane is used to turn the ladle over and pour slag. The ladle is tilted and left to stand for 1 minute. If no slag flows out, it is considered that the slag in the ladle is completely poured out, and then the 7# ladle is placed on the saddle seat for hot repair. After the nozzle burning operation is completed, hot patching materials are added in batches from both sides of the ladle mouth to the slag groove position of the slag pouring surface. After 8 batches of hot patching materials are added, it is found that the hot patching materials in the slag groove are flush with the adjacent slag line bricks, and the feeding is stopped, and then the nozzle replacement operation is performed. Since the nozzle replacement operation takes 15-20 minutes, the hand-thrown hot patching material can be completely sintered. When the molten steel from this batch was put into the LF refining furnace for treatment again, the operator was coordinated to make the slag appropriately sticky to reduce the erosion of the hot patch material on the slag groove. Through on-site observation, the hot patch material of 19 batches can last for about 10 batches. The ladle has a service life of 60 times, which is 7 times longer than the unrepaired ladle. The method of using hand-thrown hot patch material to quickly repair the slag groove can be repeatedly implemented and can effectively delay the erosion of the ladle slag line.

[0025] Example 2

[0026] This embodiment provides an online hot patching method for a ladle. The online ladle 1# has a ladle age of 35 times, and grooves are eroded at the slag line of the slag pouring surface. The depth of the slag grooves is measured to be 60 mm. The time for replacing the water nozzle at the 36th time is selected to perform rapid hot patching on the slag grooves of the slag pouring surface.

[0027] In this embodiment, magnesium oxide accounts for 77.01wt% of the total mass of the hot patch material, C accounts for 14.22wt% of the total mass of the hot patch material, aluminum oxide accounts for 5.23wt% of the total mass of the hot patch material, the binder accounts for 3.14wt% of the total mass of the hot patch material, and the moisture content is 0.40wt%. After the 36th furnace is poured, the ladle is turned over and the slag is removed by a crane. If the ladle is tilted and left to stand for 1 minute without slag flowing out, it is considered that the slag in the ladle is completely removed, and then the 1# ladle is placed on the saddle seat for hot repair.

[0028] After the nozzle burning operation is completed, the material is quickly fed from both sides of the ladle mouth to the slag groove position of the slag pouring surface. After 15 batches of hot patching materials are put in, it is found that the hot patching material in the slag groove is flush with the adjacent slag line bricks, and the feeding is stopped, and then the nozzle replacement operation is carried out. Since the nozzle replacement operation takes 15-20 minutes, the hand-thrown hot patching material can be completely sintered. When the molten steel of this batch is received and sent to the LF refining furnace for processing again, the operator is coordinated to make the slag appropriately viscous to reduce the scouring of the hot patching material in the slag groove. Through on-site observation, the hot patching material of 36 batches can last for about 7 batches. The ladle age of this ladle is 58 times, which is 5 times longer than the life of the unrepaired ladle. The method of using hand-thrown hot patching material to quickly repair the slag groove can be implemented repeatedly, which can effectively delay the erosion of the ladle slag line.

Claims

1. A method for online hot patching of a ladle, characterized in that: The steps include: S1. Determine the ladle to be repaired and the repair heat according to the slag groove depth of the ladle; S2. After the ladle is turned over and the slag is emptied, it is laid flat and hot patching material is added into the slag groove; S3. After the hot patch material is put into the ladle, ensure that the slag is viscous during the next refining.

2. The method according to claim 1, characterized in that In step S1, When the depth of the ladle slag groove is less than 60mm, repair should be postponed for one or two furnaces; When the depth of the ladle slag groove is between 60mm and 100mm, repairs should be carried out immediately for the next batch after the operation of the current batch is completed.

3. The method according to claim 1, characterized in that In step S2, when the ladle is slag-drained, the ladle is tilted and left to stand for 1 minute. If no slag flows out, it is considered that the slag in the ladle is completely drained, and the subsequent heat-adding and feeding operation is carried out.

4. The method according to claim 1, characterized in that In step S2, the hot patch material is composed of magnesium oxide, aluminum oxide, carbon, a binder and water, wherein magnesium oxide accounts for ≥76wt% of the total mass of the hot patch material, carbon accounts for ≥14wt% of the total mass of the hot patch material, aluminum oxide accounts for ≥5wt% of the total mass of the hot patch material, the binder accounts for ≥3wt% of the total mass of the hot patch material, the moisture content of the hot patch material is ≤1.0wt%, and the particle size of the hot patch material is 1mm-5mm.

5. The method according to claim 4, characterized in that The binder consists of equal amounts of modified asphalt and phenolic resin.

6. The method according to claim 1, characterized in that In step S2, hot patching material is added to make the slag groove flush with the slag line bricks adjacent to the slag groove in the ladle.