Metal ceramic composite binding agent diamond grinding wheel disc and preparation method and application thereof
Through the preparation of the diamond grinding wheel disc of the metal cermet composite bonding agent, the coordinated preparation of diamond agglomerated abrasives and Cu3Sn powder, combined with sodium sulfate and quenching treatment, the existing diamond grinding wheel is solved inadequate sharpness and service life in the process of thinning silicon carbide wafers. The short problem achieves efficient and long-life grinding wheel performance, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411149618.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
The existing diamond grinding wheels have problems such as insufficient sharpness, short service life, and easy to cause grinder load alarms and chip fragmentation in the process of thinning silicon carbide wafers. Relying on imported materials leads to high costs and long lead time, which affects domestic silicon carbide. The development of the chip industry.
The preparation method of diamond grinding wheel disc is adopted by the metal cermet composite bonding agent. Through the coordinated preparation of diamond agglomerated abrasive, Cu3Sn powder and SiO2 sol, combined with the use of sodium sulfate, a high-sharp and long service life grinding wheel is formed to avoid chip edge collapse and crushing. The uniformity and strength of Cu3Sn are improved by quenching treatment.
It realizes the high sharpness, long service life and low surface roughness of diamond grinding wheels in the process of thinning silicon carbide wafers, improves processing efficiency, avoids wafer edge collapse and fragmentation, and is suitable for large-scale industrial production.
Smart Images

Figure CN118927170A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a metal-ceramic composite binder diamond grinding wheel disc and a preparation method and application thereof, belonging to the field of abrasive material and tool manufacturing. Background Art
[0002] SiC belongs to the third generation of semiconductor materials. Compared with the semiconductor material Si, its bandgap is 2.9 times that of Si, its saturated electron drift rate is 2 times that of Si, its breakdown voltage is about 12 times that of Si, and its thermal conductivity is about 2.7 times that of Si. Therefore, SiC materials have been widely used in high-voltage and high-frequency fields such as high-power charging piles and radar base stations. At the same time, as a typical hard and brittle material, SiC has a Mohs hardness of up to 9.5, and high requirements are placed on the surface accuracy and surface quality during thinning, which puts forward quite high requirements on the diamond grinding wheel used for thinning.
[0003] At present, most of the rough and fine grinding diamond wheels used in the market rely on imports from Japan and the United States. They are expensive, have long delivery cycles, and are difficult to adapt to domestic grinding machines, which has affected the rapid development of the domestic silicon carbide wafer industry. Domestic research has been conducted on resin-bonded diamond wheels, ceramic-bonded diamond wheels, and metal-bonded diamond wheels for thinning silicon carbide wafers. However, resin-bonded diamond wheels are prone to burns and tooth loss; ceramic-bonded diamond wheels have a low service life; and metal-bonded diamond wheels are not sharp enough, which can easily lead to problems such as grinder load alarms and wafer breakage. Summary of the invention
[0004] In view of the shortcomings of the existing silicon carbide wafer thinning technology, the first purpose of the present invention is to provide a method for preparing a metal-ceramic composite binder diamond grinding wheel. The preparation method of the present invention is simple and controllable and suitable for large-scale industrial production.
[0005] The second object of the present invention is to provide a metal-ceramic composite binder diamond grinding wheel disc prepared by the above-mentioned preparation method. The diamond grinding wheel disc prepared by the present invention has high porosity of diamond grinding wheel teeth, strong chip holding and chip removal capacity, good sharpness, high processing efficiency, long service life, and low surface roughness of silicon carbide wafer after thinning.
[0006] The third object of the present invention is to provide an application of a metal-ceramic composite binder diamond grinding wheel disc prepared by the above-mentioned preparation method. The diamond grinding wheel disc provided by the present invention is used for thinning silicon carbide wafers. SiC is a typical hard and brittle material. The Mohs hardness of up to 9.5 makes the traditional grinding wheel wear fast, and the high brittleness easily leads to chip edge collapse and fragmentation during the grinding process. The diamond grinding wheel disc prepared by the present invention uses diamond agglomerated abrasive as an abrasive. The diamond agglomerated abrasive is a small ball formed by agglomerating diamond micropowder and a ceramic binder, and is synergistically prepared by adding a metal binder Cu3Sn and a SiO2 sol (equivalent to a ceramic binder). Therefore, the metal grinding wheel has good shape retention and a high sharpness of a ceramic grinding wheel. When grinding SiC materials, the Cu3Sn binder ensures that the grinding wheel has a long service life, and the diamond agglomerated abrasive and the SiO2 sol ensure the high sharpness of the grinding wheel, thereby avoiding chip edge collapse and fragmentation. At the same time, the pores prepared by sodium sulfate ensure that the grinding wheel has excellent chip holding and chip removal capabilities.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme:
[0008] The invention discloses a method for preparing a metal-ceramic composite binder diamond grinding wheel disc for thinning silicon carbide wafers. The method comprises the following steps: mixing diamond agglomerated abrasive, Cu3Sn powder and sodium sulfate to obtain mixed powder; mixing the mixed powder with SiO2 sol and then granulating the mixed powder to obtain mixed particles; hot pressing and sintering the mixed particles to obtain a sintered green body; quenching the sintered green body to obtain diamond grinding wheel teeth; and combining the diamond grinding wheel teeth with an aluminum matrix to obtain a diamond grinding wheel disc.
[0009] The diamond grinding wheel teeth of the present invention use diamond agglomerated abrasive as abrasive. The diamond agglomerated abrasive is a small ball formed by agglomerating diamond micropowder and a ceramic binder. The diamond agglomerated abrasive has good self-sharpening property and continuously generates new cutting edges through self-crushing during the grinding process, thereby making the diamond grinding wheel have high sharpness and improving the grinding quality of the grinding wheel. However, the existing Fe-based and bronze-based binders are poorly bonded to the ceramic-based agglomerated abrasive. The present invention uses Cu3Sn as a binder, which has a softening temperature close to that of the agglomerated abrasive. During hot pressing, the melted Cu3Sn can wet the softened diamond agglomerated abrasive well, thereby ensuring good bonding strength between Cu3Sn and the diamond agglomerated abrasive. In addition, SiO2 sol is added as a wetting agent for granulation, and can also be used as a ceramic binder to further improve the bonding between Cu3Sn and the agglomerated abrasive. In addition, sodium sulfate is added as a pore-forming agent. Sodium sulfate will not decompose during sintering, has stable properties, and is soluble in water. During the grinding process, the sodium sulfate in the grinding wheel dissolves in the water-based grinding fluid to form pores. On the one hand, the pores can accommodate the grinding chips generated during the grinding process, and the grinding wheel is not easily blocked; on the other hand, the pores can accommodate the coolant to promptly take away the heat generated during the grinding process; in addition, the diamonds that fall off during grinding can be accommodated in the pores to avoid rolling on the grinding surface and causing scratches.
[0010] During the preparation process, the present invention further performs quenching treatment after sintering. The inventors found that the quenching treatment can make the Cu3Sn metal binder composition more uniform, while producing grain refinement, improving strength, and increasing the holding force of Cu3Sn on the abrasive, thereby increasing the service life of the grinding wheel. On the other hand, the agglomerated abrasive is more brittle after water quenching, and the diamond is evenly peeled off during the grinding process, so that the grinding wheel has good self-sharpening properties.
[0011] Therefore, under the coordination of components and processes, the diamond grinding wheel obtained by the present invention can have good sharpness, high processing efficiency, long service life when thinning SiC wafers, and the surface roughness of the silicon carbide wafer after thinning is low.
[0012] The inventors found that only diamond agglomerated abrasives can ensure sharpness, because agglomerated abrasives are small balls formed by agglomeration of diamond micropowder and ceramic binder. The ceramic binder is highly brittle, and during the grinding process, the agglomerated abrasive will self-break to reveal new diamond cutting edges. In the actual exploration process, the inventors also tried to use diamond micropowder, but after the diamond micropowder was blunted, the metal binder had a strong grip on the diamond and could not fall off in time, resulting in insufficient sharpness of the grinding wheel.
[0013] In a preferred solution, the mixed powder is composed of the following by mass percentage: diamond agglomerated abrasive: 15-20%; Cu3Sn powder: 60-70%; sodium sulfate: 10-20%. In the present invention, the amount of each component in the mixed powder is controlled within the scope of the present invention, and the performance is optimal. However, if too much diamond agglomerated abrasive is added, the strength of the grinding wheel will be too low and the wear resistance will deteriorate; if too little is added, the cutting edge will be insufficient, resulting in insufficient sharpness of the grinding wheel. Too much Cu3Sn powder will result in too high strength of the grinding wheel and insufficient sharpness; too little will result in too low strength of the grinding wheel and easy tooth breakage during grinding.
[0014] In a preferred solution, the diamond agglomerated abrasive is spherical in shape and has a particle size of 20-30 μm. The inventors have found that the use of spherical diamond agglomerated abrasive can make the surface roughness of silicon carbide ground by diamond grinding wheel smaller.
[0015] In addition, the inventors found that controlling the particle size of the diamond agglomerated abrasive to 20-30 μm can achieve the best grinding quality for silicon carbide, good surface quality of silicon carbide and high grinding efficiency. If the particle size of the diamond agglomerated abrasive is too small, the sharpness of the grinding wheel is insufficient. If the particle size is too large, the agglomerated abrasive is easy to break, resulting in excessive surface roughness of the silicon carbide.
[0016] In a preferred embodiment, the diamond agglomerated abrasive is a sphere formed by agglomerating 5-10 μm diamonds with a ceramic binder.
[0017] In a preferred embodiment, the particle size of the sodium sulfate is 50-100 μm.
[0018] The inventors have found that the particle size of sodium sulfate has a certain influence on the performance of the final material. If the sodium sulfate particles are too large or the content is too high, the mechanical properties of the diamond grinding wheel teeth will drop sharply, the shape retention of the grinding wheel will deteriorate, and even problems such as edge collapse may occur during the grinding process. If the particle size of sodium sulfate is too small or the content is too little, it will not have an effective cooling effect.
[0019] The preferred solution is to mix diamond agglomerated abrasive, Cu3Sn powder and sodium sulfate, and then pass the mixture through a 200-mesh sieve to obtain the sieve residue, and then place the sieve residue in a V-type mixer to mix the mixture to obtain a mixed powder. The speed during mixing is controlled to be 90-120 r / min, and the mixing time is 24-36 h.
[0020] The inventors have found that after the raw material powders are preliminarily mixed, the sieved material is sieved once and then mixed again, so that the mixing can be more uniform and the density of the final material can be higher.
[0021] In a preferred embodiment, the SiO2 sol is a neutral SiO2 sol, and the SiO2 particles in the SiO2 sol are nanometer-sized.
[0022] In a preferred embodiment, the mass fraction of SiO2 particles in the SiO2 sol is 15-20%.
[0023] In a preferred embodiment, the amount of SiO2 sol added is 3-5% of the mass of the mixed powder. If the amount of SiO2 sol added is controlled within the above range, the mixed particles produced are the most uniform and have the best performance, so that the performance of the final grinding wheel is the best.
[0024] The preferred solution is to mix the mixed powder with SiO2 sol, squeeze through a 20-mesh screen, and dry to obtain mixed particles. In the actual operation process, nano-SiO2 sol is added to the mixed powder, stirred and impregnated, and squeezed through a 20-mesh screen, and then dried. The drying temperature is controlled to be 80°C and the drying time is more than 4 hours.
[0025] In a preferred embodiment, the hot pressing sintering process is as follows: firstly, the temperature is increased to 300-450°C at a heating rate of 15-25°C / min, and kept at this temperature for 20-40min; then, the temperature is increased to 600-650°C at a heating rate of 10-15°C / min, and kept at this temperature for 60-90min; and the pressure of the hot pressing sintering is 20-25MPa.
[0026] In actual operation, the mixed particles are loaded into a graphite mold for hot pressing and sintering, and the hot pressing and sintering is performed under a nitrogen atmosphere.
[0027] The inventors found that a hot pressing temperature that is too high will cause the diamond agglomerated abrasive to deform, while a hot pressing temperature that is too low will cause the grinding wheel teeth to be insufficiently strong and easy to break.
[0028] In a preferred embodiment, the quenching process is as follows: placing the sintered body in a furnace preheated to 480-500°C, heating it to 580-600°C, keeping it at that temperature for 60-120 minutes, and then water cooling it to room temperature.
[0029] Further preferably, the furnace is preheated to 480-500°C at a heating rate of 20-30°C / min, and then the sintered green body is placed in the preheated furnace and heated to 580-600°C at a rate of 5-10°C / min. In the actual operation, after the quenching treatment and heat preservation are completed, it is quickly cooled to room temperature with water at a water temperature of 20°C.
[0030] In the present invention, quenching treatment is performed. On the one hand, the composition of the Cu3Sn metal binder is made more uniform, and at the same time, grain refinement is produced, strength is improved, and the holding force of Cu3Sn on the abrasive is increased, thereby increasing the service life of the grinding wheel. On the other hand, the agglomerated abrasive is more brittle after water quenching, and diamonds are evenly peeled off during the grinding process, so that the grinding wheel has good self-sharpening properties.
[0031] In a preferred solution, the diamond grinding wheel teeth are combined with the aluminum substrate by gluing the diamond grinding wheel teeth to the aluminum substrate and then curing the diamond grinding wheel teeth.
[0032] The present invention also provides a metal-ceramic composite binder diamond grinding wheel disc prepared by the preparation method.
[0033] The present invention also provides an application of a metal-ceramic composite binder diamond grinding wheel disc prepared by the above preparation method, and the diamond grinding wheel disc is applied to thinning silicon carbide wafers.
[0034] Beneficial effects:
[0035] 1. The present invention uses diamond agglomerated abrasives, which are composed of multiple small diamonds bonded by a ceramic binder. During the grinding process, the agglomerated abrasives continuously undergo brittle fractures to achieve self-sharpening, and new cutting edges are continuously exposed, so that the grinding wheel has good self-sharpening and sharpness. The surface roughness of the processed silicon carbide is lower.
[0036] 2. The nano-SiO2 sol is selected as a wetting agent in the present invention, which improves the bonding between Cu3Sn and the agglomerated abrasive and increases the holding force of Cu3Sn on the agglomerated abrasive. At the same time, sodium sulfate is used as a pore-forming agent to improve the chip holding and chip removal capabilities of the grinding wheel.
[0037] 3. The present invention can make the composition of the Cu3Sn metal binder more uniform by heat treatment strengthening, and at the same time produce grain refinement and improve strength. The holding force of Cu3Sn on the abrasive is increased, thereby increasing the service life of the grinding wheel. On the other hand, the agglomerated abrasive is more brittle after water quenching, and the diamond is evenly peeled off during the grinding process, so that the grinding wheel has good self-sharpening properties.
[0038] In summary, under the coordination of components and processes, the diamond grinding wheel obtained by the present invention can have good sharpness, high processing efficiency, long service life when thinning SiC wafers, and the surface roughness of the silicon carbide wafer after thinning is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] 1. Figure 1 This is a physical picture of the grinding wheel in the embodiment of the present invention.
[0040] 2. Figure 2 4 is a structural diagram of a grinding wheel in an embodiment of the present invention.
[0041] 3. Figure 3 This is the microscopic morphology of the grinding wheel teeth in the embodiment of the present invention. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described in detail below in conjunction with the embodiments, but the protection scope of the invention is not limited thereto.
[0043] The diamond agglomerated abrasives in the following examples were purchased from Hunan Maxfield New Materials Technology Co., Ltd.
[0044] Example 1
[0045] The process steps are:
[0046] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0047] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0048] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0049] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0050] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0051] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 minutes, and then water cool to room temperature.
[0052] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0053] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0054] Example 2
[0055] The process steps are:
[0056] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0057] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 15ωt.% 70ωt.% 15ωt.%
[0058] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0059] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0060] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0061] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 minutes, and then water cool to room temperature.
[0062] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0063] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0064] Example 3
[0065] The process steps are:
[0066] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0067] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0068] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0069] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0070] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 600°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0071] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 minutes, and then water cool to room temperature.
[0072] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0073] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0074] Example 4
[0075] The process steps are:
[0076] 1. Prepare the raw materials according to the composition ratio in the table below, mix them, pass them through a 200-mesh sieve, take the undersize, and then mix the undersize in a V-type mixer at a speed of 120 r / min for 24 h to prepare a uniform powder mixture.
[0077] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0078] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0079] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0080] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 650°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0081] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 min, and then water cool to room temperature.
[0082] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0083] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0084] Comparative Example 1
[0085] The process steps are:
[0086] 1. Prepare the raw materials according to the composition ratio in the table below, mix them, pass them through a 200-mesh sieve, take the undersize, and then mix the undersize in a V-type mixer at a speed of 120 r / min for 24 h to prepare a uniform powder mixture.
[0087] Components Diamond powder <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0088] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0089] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0090] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0091] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 min, and then water cool to room temperature.
[0092] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0093] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0094] Comparative Example 2
[0095] The process steps are:
[0096] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0097] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0098] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0099] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0100] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0101] 4. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0102] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0103] Comparative Example 3
[0104] The process steps are:
[0105] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0106] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> Sodium sulfate Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0107] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0108] 2. Add 5ωt.% of liquid paraffin to the powder mixture, stir evenly, sieve, granulate and load into graphite mold.
[0109] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0110] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 minutes, and then water cool to room temperature.
[0111] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0112] Comparative Example 4
[0113] The process steps are:
[0114] 1. Prepare the raw materials according to the composition ratio in the table below, mix, pass through a 200-mesh sieve, take the sieve-down material, and then mix the sieve-down material in a V-type mixer at a speed of 120 r / min for 24 hours to prepare a uniform powder mixture.
[0115] Components Diamond Agglomerated Abrasive <![CDATA[Cu3Sn powder]]> graphite Mass percentage 20ωt.% 65ωt.% 15ωt.%
[0116] The particle size of the diamond agglomerated abrasive used is 20-30 μm, and the particle size of the sodium sulfate used is 50-100 μm.
[0117] 2. Add 5ωt.% of nano-SiO2 sol to the powder mixture, stir evenly, sieve, granulate, dry at 80℃ and then put into graphite mold.
[0118] 3. The mold was placed in a graphite hot press, and the temperature was first raised to 400°C at a heating rate of 20°C / min, and kept at that temperature for 30 minutes, and then raised to 620°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes. The hot press pressure was 25 MPa.
[0119] 4. Preheat the muffle furnace to 500°C, place the grinding wheel teeth in the furnace, heat to 600°C, keep warm for 90 minutes, and then water cool to room temperature.
[0120] 5. After grinding the grinding wheel teeth to a certain size, glue them to the aluminum substrate with AB type epoxy resin. After curing for 24 hours, the diamond grinding wheel is obtained.
[0121] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0122] The diamond grinding wheel prepared according to the above method was used to grind silicon carbide wafers for performance testing. The test results are shown in Table 1.
[0123] Table 1 Performance of diamond grinding wheels prepared in Examples and Comparative Examples
[0124]
[0125]
Claims
1. A method for preparing a metal-ceramic composite bond diamond grinding wheel, characterized in that: Diamond agglomerated abrasive, Cu3Sn powder and sodium sulfate are mixed to obtain mixed powder, the mixed powder is mixed with SiO2 sol and then granulated to obtain mixed particles, the mixed particles are hot-pressed and sintered to obtain a sintered green body, the sintered green body is quenched to obtain diamond grinding wheel teeth, and the diamond grinding wheel teeth are combined with an aluminum matrix to obtain a diamond grinding wheel disc.
2. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1, characterized in that: The mixed powder is composed of the following by mass percentage: diamond agglomerated abrasive: 15-20%; Cu3Sn powder: 60-70%; sodium sulfate: 10-20%; The diamond agglomerated abrasive is spherical in shape and has a particle size of 20-30 μm.
3. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: The diamond agglomerated abrasive is a sphere formed by agglomerating 5-10 μm diamonds and a ceramic binder; The particle size of the sodium sulfate is 50-100 μm.
4. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: Diamond agglomerated abrasive, Cu3Sn powder and sodium sulfate are mixed and passed through a 200-mesh sieve to obtain the sieve residue, and then the sieve residue is placed in a V-type mixer to mix the mixture to obtain mixed powder. The speed during mixing is controlled to be 90-120 r / min and the mixing time is 24-36 hours.
5. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: The SiO2 sol is a neutral SiO2 sol, and the SiO2 particles in the SiO2 sol are nanometer-sized; In the SiO2 sol, the mass fraction of SiO2 particles is 15-20%; The added amount of the SiO2 sol is 3-5% of the mass of the mixed powder.
6. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: After mixing the mixed powder with SiO2 sol, the mixed powder is squeezed through a 20-mesh screen and dried to obtain mixed particles; The hot pressing sintering process is: firstly heating to 300-450°C at a heating rate of 15-25°C / min, keeping the temperature for 20-40min, then heating to 600-650°C at a heating rate of 10-15°C / min, keeping the temperature for 60-90min, and the pressure of the hot pressing sintering is 20-25MPa.
7. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: The quenching process is as follows: placing the sintered green body in a furnace preheated to 480-500° C., heating it to 580-600° C., keeping it warm for 60-120 minutes, and then cooling it to room temperature with water.
8. The method for preparing a metal-ceramic composite bond diamond grinding wheel according to claim 1 or 2, characterized in that: The diamond grinding wheel teeth are combined with the aluminum substrate by gluing the diamond grinding wheel teeth onto the aluminum substrate and then curing the gluing.
9. A metal-ceramic composite bond diamond grinding wheel prepared by the preparation method according to any one of claims 1 to 8.
10. Application of a metal-ceramic composite bond diamond grinding wheel prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The diamond grinding wheel is applied to silicon carbide wafer thinning.
Citation Information
Patent Citations
Metal ceramic combination binding agent and combination binding agent diamond wheel
CN103831740A
Ceramic metal composite binding agent grinding wheel and preparation method thereof
CN110842799A
Grinding wheel for magnetic material polishing and preparation method thereof
CN117601031A
Grinding tool, especially cutting-off tool and method of manufacturing such a tool
EP0744247A1
Cited By
Agglomerated diamond powder and preparation method thereof
CN121374446A