Biomass hard carbon material, preparation method and application thereof, sodium ion battery negative pole piece containing biomass hard carbon material, and sodium ion battery

The treatment of biomass raw materials through solid phase method has solved the problem of difficult control of ion doping amount and wastewater pollution in the prior art, and improved the capacity and first effect of biomass hard carbon materials, which are suitable for the negative electrode sheet of sodium ion battery.

CN118929631AInactive Publication Date: 2024-11-12四川易纳能新能源科技有限公司

Patent Information

Application Number
CN202411172929.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the application of sodium ion battery negative electrodes, existing biomass hard carbon materials have problems such as difficult to control the ion doping amount, large amount, high cost, and wastewater pollution, resulting in insufficient electrochemical performance.

Method used

The biomass raw materials are pre-carbonized and decomposed by solid phase method, and then solid phase mixing with ionic compounds and carbonized at high temperatures to reduce the amount of ionic compounds, accurately control the doping amount, and form high-performance biogenesis. Material hard carbon material.

Benefits of technology

It realizes efficient production of ion doping, reduces costs, avoids wastewater pollution, improves the capacity and first-effect of biomass hard carbon materials, and is suitable for sodium ion battery negative electrode sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929631A_ABST
    Figure CN118929631A_ABST
Patent Text Reader

Abstract

The invention provides a biomass hard carbon material, a preparation method and application thereof, a sodium ion battery negative electrode plate containing the biomass hard carbon material, and a sodium ion battery, and relates to the technical field of sodium ion battery negative electrode materials. According to the preparation method of the biomass hard carbon material, most biomass components in the biomass raw material overflow in the form of small molecule gas through pre-carbonization treatment, so that a stable carbon frame structure is obtained; and mixing the hard carbon precursor obtained after impurity removal with an ionic compound solid phase, and carbonizing to obtain the biomass hard carbon material. Through detection, the preparation method of the biomass hard carbon material can achieve the effects of accurately controlling the ion doping amount and greatly reducing the dosage of the ionic compound, meanwhile, the ion doping production efficiency is improved, the doping cost is reduced, and waste liquid pollution in the liquid phase doping process is also avoided. The biomass hard carbon material has the technical effects of high capacity and high first efficiency, and can be widely applied to the preparation process of the negative pole piece of the sodium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new negative electrode materials, and in particular to a biomass hard carbon material, a preparation method and application thereof, and a sodium ion battery negative electrode sheet and a sodium ion battery containing the same. Background Art

[0002] As one of the potential application batteries for energy storage systems and low-speed electric vehicles, sodium-ion batteries have gained widespread attention in the market due to their low cost advantage. In recent years, research on sodium batteries has become increasingly popular, but the disadvantage of sodium batteries is their low energy density. In order to improve this situation, the development of high-performance positive and negative electrode materials has become the mainstream direction of sodium-ion battery development.

[0003] As for the negative electrode material of sodium-ion batteries, although there are many types of materials that can be used as negative electrodes, carbon materials with low cost and excellent electrochemical performance have been commercialized first in the negative electrodes of sodium-ion batteries at this stage, among which hard carbon is more suitable for the development and application of sodium negative electrodes. Due to the many sources and synthesis methods of hard carbon, from the perspectives of material source, cost, and process, biomass hard carbon has become the first choice for most sodium negative electrode manufacturers, and most of the hard carbon on the market belongs to biomass hard carbon.

[0004] At present, biomass hard carbon has problems such as low first efficiency and reversible capacity. To address this phenomenon, the performance can be improved by combining soft and hard carbon, ion doping, electrolyte modification, etc. Among them, ion doping can achieve a large degree of capacity improvement, but the disadvantage is that the first efficiency is relatively low. In response to this phenomenon, CN114497543A modified polysaccharide biomass by liquid metal ion impregnation, followed by high-temperature carbonization to obtain high-performance biomass hard carbon; CN117894967A used a large amount of biomass raw materials as a carbon source, increased the active sites of metal ion doping by removing impurities to improve electrochemical performance, and developed a modification method that is more suitable for a large amount of biomass hard carbon, but both methods have the problem of large amounts of doped ion compounds, unable to accurately control the amount of ion doping, cumbersome processing, long processing time, high energy consumption, and a large amount of wastewater pollution, and are limited in mass production and manufacturing processes.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide a method for preparing biomass hard carbon materials. Compared with liquid phase ion doping, the method for preparing biomass hard carbon materials can achieve the effect of accurately controlling the amount of ion doping and greatly reducing the amount of ionic compounds used, thereby improving the ion doping production efficiency and reducing the doping cost. At the same time, it avoids the risk of low liquid phase doping efficiency and the generation of a large amount of wastewater that is easy to pollute the environment.

[0007] The second object of the present invention is to provide a biomass hard carbon material, which is prepared by the above-mentioned preparation method and has the advantages of high capacity and high initial efficiency compared with existing biomass hard carbon materials.

[0008] The third object of the present invention is to provide an application of the above-mentioned biomass hard carbon material.

[0009] The fourth object of the present invention is to provide a negative electrode plate for a sodium ion battery.

[0010] A fifth object of the present invention is to provide a sodium ion battery.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0012] The biomass raw material is pre-carbonized and then impurities are removed to obtain a hard carbon precursor; the hard carbon precursor is then mixed with an ionic compound using a solid phase method, and the solid phase mixed material is subjected to a high temperature carbonization treatment to obtain a biomass hard carbon material;

[0013] The temperature of the pre-carbonization treatment is 400-800°C, the holding time is 2-6h, and the heating rate is 2-10°C / min;

[0014] In the solid phase mixing process, the mass ratio of the hard carbon precursor to the ionic compound is 1:0.01-0.3, and the particle size D50 of the hard carbon precursor is 2-20 μm.

[0015] Further, the biomass raw material includes at least one of peanut shells, bamboo, walnut shells, coconut shells, almond shells, waste wood, rice husks and wheat husks;

[0016] And / or, the biomass raw material includes at least one of glucose, starch, cellulose and lignin.

[0017] Further, the pre-carbonization treatment is carried out under a protective gas atmosphere;

[0018] Preferably, the protective gas includes any one or more of nitrogen, argon, helium or hydrogen.

[0019] Furthermore, the impurity removal is impurity removal with an acid solution;

[0020] Preferably, the step of crushing the pre-carbonized biomass raw material is further included before the impurity removal, and the D50 of the crushed material is 50 μm to 2 mm.

[0021] Preferably, the acid solution includes at least one of hydrochloric acid solution, sulfuric acid solution, nitric acid solution, oxalic acid, and citric acid solution;

[0022] More preferably, the acid solution has a concentration of 0.1 to 5 mol / L;

[0023] Preferably, during the impurity removal process, the solid-to-liquid ratio of the pre-carbonized biomass raw material to the acid solution is 1:10-30;

[0024] Preferably, the impurity removal method comprises: mixing the pre-carbonized biomass raw material and the acid solution and dispersing them at 30 to 60° C. for 0.5 to 12 hours, and then washing them with deionized water for at least 5 times until they are neutral, to obtain a hard carbon precursor;

[0025] Furthermore, the ion mixture and the impurity-removing precursor are solid-phase mixed, and the ionic compound includes a non-metallic compound and a metal ion compound;

[0026] Preferably, the non-metallic compound includes at least one of urea, thiourea, ammonium chloride, melamine, and diammonium phosphate;

[0027] Preferably, the metal ion compound includes at least one of nitrates, phosphates and metal chlorides containing the metal elements manganese, zinc and iron.

[0028] Furthermore, the pyrolysis temperature of the high-temperature carbonization treatment is 1000-1600° C., the pyrolysis treatment time is 2-6 hours, and the heating rate of the pyrolysis treatment is 1-5° C. / min.

[0029] The present invention provides a biomass hard carbon material, which is mainly prepared by the above-mentioned method for preparing the biomass hard carbon material.

[0030] The present invention provides an application of the above-mentioned biomass hard carbon material in preparing a negative electrode plate for a sodium ion battery.

[0031] The present invention provides a sodium ion battery negative electrode plate, wherein the component raw materials of the sodium ion battery negative electrode plate include, by mass percentage:

[0032] 90-95% of biomass hard carbon material, 1-5% of conductive carbon black, and 1-5% of polyvinylidene fluoride.

[0033] The present invention provides a sodium ion battery, which comprises the above-mentioned sodium ion battery negative electrode plate.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention provides a method for preparing a biomass hard carbon material, wherein the preparation method first pre-carbonizes the biomass raw material, then removes impurities, and obtains a hard carbon precursor; then the hard carbon precursor is mixed with an ionic compound by a solid phase method, and the mixed material is subjected to a high-temperature carbonization treatment to obtain a biomass hard carbon material. The preparation method of the present application can allow most of the biomass components in the biomass raw material to overflow in the form of small molecule gases through a pre-carbonization treatment process of keeping warm for 2 to 6 hours at 400 to 800°C, thereby obtaining a stable carbon framework structure; then the hard carbon precursor obtained after impurities removal is mixed with an ionic compound in a solid phase and then subjected to a carbonization treatment to obtain a biomass hard carbon material.

[0036] After testing, the preparation method of the biomass hard carbon material of the present application can greatly reduce the amount of ionic compounds used. The mass ratio of the hard carbon precursor to the ionic compound in the solid phase carbonization process is only 1:0.01~0.3; at the same time, the solid phase carbonization treatment method also greatly reduces the mixing modification time of ion doping modification, reduces the difficulty of treatment, and utilizes the liquefaction and sublimation phenomenon of ionic compounds in the heating process. The biomass hard carbon is infiltrated and coated by liquefaction. The sublimated ions overflow from the inside of the hard carbon in a gaseous state to modify the material structure, thereby improving the affinity for sodium ions, improving conductivity, optimizing the interlayer spacing, and improving the sodium storage capacity of the hard carbon, thereby improving the reversible capacity of the hard carbon; and through the controllable regulation of the amount of doped ions, the problem of too many irreversible defects in the hard carbon due to high ion doping is effectively avoided, thereby obtaining a high-capacity and first-effect biomass hard carbon material to meet the needs of the negative electrode of the sodium ion battery, and effectively avoiding the existing biomass hard carbon liquid phase doping treatment process. The large amount of ionic compounds used, low doping efficiency, cumbersome doping process, high energy consumption, and a large amount of wastewater pollution generated during the treatment process.

[0037] The biomass hard carbon material provided by the present invention can be widely used in the preparation process of the negative electrode sheet of a sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 The first charge and discharge curves of Example 1, Example 6 and Comparative Example 3 provided in Test Example 1 of the present invention;

[0040] Figure 2Cycling performance diagram of Example 1, Example 6 and Comparative Example 3 provided in Test Example 1 of the present invention at 1C rate;

[0041] Figure 3 X-ray diffraction patterns of Example 1, Example 6, and Comparative Example 3 provided in Test Example 1 of the present invention;

[0042] Figure 4 The scanning electron microscope image of Example 1 provided for Experimental Example 2 of the present invention;

[0043] Figure 5 The scanning electron microscope image of Example 6 provided for Experimental Example 2 of the present invention;

[0044] Figure 6 The scanning electron microscope image of the comparative example 3 provided for the experimental example 2 of the present invention;

[0045] Figure 7 Thermogravimetric curves of the ionic compounds (zinc chloride, ammonium chloride, melamine) used in Example 1, Example 6, and Comparative Example 3 provided in Test Example 2 of the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] According to one aspect of the present invention, a method for preparing a biomass hard carbon material comprises:

[0048] The biomass raw material is pre-carbonized and then impurities are removed to obtain a hard carbon precursor; the hard carbon precursor is then solid-phase mixed with an ionic compound using a solid-phase method, and the mixed material is subjected to high-temperature carbonization to obtain a biomass hard carbon material;

[0049] The temperature of the pre-carbonization treatment is 400-800°C, the holding time is 2-6h, and the heating rate is 2-10°C / min;

[0050] In the solid phase mixing process, the mass ratio of the hard carbon precursor to the ionic compound is 1:0.01-0.3, and the particle size D50 of the hard carbon precursor is 2-20 μm.

[0051] The present invention provides a method for preparing a biomass hard carbon material, wherein the preparation method first pre-carbonizes the biomass raw material, then removes impurities, and obtains a hard carbon precursor; then the hard carbon precursor is mixed with an ionic compound by a solid phase method, and the mixed material is subjected to a high-temperature carbonization treatment to obtain a biomass hard carbon material. The preparation method of the present application can allow most of the biomass components in the biomass raw material to overflow in the form of small molecule gases through a pre-carbonization treatment process of keeping warm for 2 to 6 hours at 400 to 800°C, thereby obtaining a stable carbon framework structure; then the hard carbon precursor obtained after impurities removal is mixed with an ionic compound in a solid phase and then subjected to a carbonization treatment to obtain a biomass hard carbon material. After testing, it was found that the preparation method of the biomass hard carbon material of the present application can greatly reduce the amount of ionic compounds used. The mass ratio of the hard carbon precursor to the ionic compound during the carbonization process is only 1:0.01~0.3; at the same time, the solid-phase carbonization treatment method also greatly reduces the mixing modification time of ion doping modification, reduces the difficulty of treatment, and can obtain high-capacity and first-effect biomass hard carbon materials, so that they can meet the needs of sodium ion battery negative electrode plates, and effectively alleviate the existing biomass hard carbon preparation process. The problems of large amount of ionic compounds, cumbersome treatment process, inefficient cycle, and wastewater pollution during the treatment process.

[0052] It should be noted that the beneficial effects of the biomass hard carbon material preparation method of the present application compared with the prior art can be summarized as follows:

[0053] (1) The present invention is pre-carbonized and de-doped before ion doping. Pre-carbonization helps to build a carbon layer framework structure, and can reduce the amount of doping compounds used and simplify the difficulty of process treatment; de-doping is conducive to removing most of the impurity elements, avoiding the reaction between the impurity elements and non-metallic compounds to affect sodium storage, and further improving the electrochemical performance;

[0054] It should be noted that the purpose of the pre-carbonization treatment in this application is to provide a biomass carbon material with a specific stable carbon framework structure. Before pre-carbonization, the biomass raw material needs to be pre-cleaned to remove impurities such as ash, soil, and stones on the surface of the biomass material that cannot be carbonized;

[0055] The purpose of using inorganic acid for impurity removal treatment is to remove soluble impurity elements in biomass carbon, avoid the chemical combination between impurity elements and doping ions affecting the normal deintercalation of sodium ions, and further increase the electrochemical properties of hard carbon.

[0056] (2) The present invention performs doping treatment on biomass hard carbon materials by doping ions during high-temperature carbonization (i.e., the hard carbon precursor is mixed with an ionic compound and carbonized by a solid-phase method), thereby improving the affinity and conductivity of biomass hard carbon for sodium ions, optimizing carbon structure information (interlayer spacing, crystal particle size, crystallinity, etc.), and thereby improving the sodium storage capacity of hard carbon and the reversible capacity of hard carbon;

[0057] Specifically, the present invention utilizes the liquefaction and sublimation of ionic compounds during the heating process, and penetrates and covers the biomass hard carbon through liquefaction. The sublimated ions overflow from the hard carbon in a gaseous state to modify the material structure, thereby improving the affinity for sodium ions, improving conductivity, optimizing interlayer spacing, and other methods to improve the sodium storage capacity of the hard carbon and the reversible capacity of the hard carbon; and through the controllable regulation of the amount of doped ions, the problem of too many irreversible defects in the hard carbon due to high ion doping is effectively avoided. The present application obtains a high-capacity and high-initial-efficiency biomass hard carbon material through this comprehensive treatment method.

[0058] (3) The present invention performs doping treatment by solid phase mixing, and the biomass hard carbon is modified by the liquefaction and gasification of ionic compounds in the high temperature section. The liquefaction penetrates the hard carbon material to adjust the hard carbon structure. When the temperature is further increased, the ionic compounds begin to gasify, and most of the doped ions inside the hard carbon begin to sublimate and overflow, resulting in an increase in the number of closed pores inside the material, thereby modifying the biomass hard carbon.

[0059] (4) Compared with the liquid phase ion doping method, solid phase doping improves the utilization rate of ion doping, improves the controllability of the doping amount of ionic compounds, and reduces the risk of uncontrollable liquid phase doping ion doping amount, thereby effectively avoiding excessive irreversible defects caused by high ion doping and ensuring the excellent electrochemical properties of biomass hard carbon; at the same time, compared with the existing metal ion doping process of hard carbon materials, the solid phase doping method of the present application improves the timeliness of the doping treatment and reduces the difficulty of doping, avoiding the pollution of the environment by the wastewater generated by liquid phase doping, and is an efficient and environmentally friendly treatment method for modified biomass hard carbon, which is more beneficial to the preparation of large quantities of materials;

[0060] The method for preparing biomass hard carbon material of the present application is described below according to the processing steps of the method.

[0061] (a) Before pre-carbonization:

[0062] In a preferred embodiment of the present invention, the biomass raw material includes at least one of peanut shells, bamboo, walnut shells, coconut shells, almond shells, waste wood, rice husks and wheat husks; and / or, the biomass raw material includes at least one of glucose, starch, cellulose and lignin.

[0063] It should be noted that the preparation method of biomass hard carbon material of the present invention is suitable for the pretreatment and modification of a wide range of bio-based materials, including but not limited to the above-mentioned optional biomass raw materials, and can effectively improve the reversible capacity and first-week coulombic efficiency of the hard carbon negative electrode material after pyrolysis.

[0064] When the biomass raw materials are peanut shells, bamboo, walnut shells, coconut shells, almond shells, waste wood, rice husks and wheat husks, they are pre-cleaned and dried in sequence before the pre-carbonization treatment to remove impurities such as ash, stones, and soil attached to the surface of the biomass that cannot be carbonized.

[0065] In a preferred embodiment of the present invention, the pre-cleaning solution is any one of deionized water and domestic water;

[0066] (II) Pre-carbonization treatment:

[0067] The biomass raw material is subjected to a pre-carbonization treatment, wherein the pre-carbonization treatment temperature is 400-800°C, the heat preservation time is 2-6 hours, and the heating rate is 2-10°C / min;

[0068] In a preferred embodiment of the present invention, the pre-carbonization treatment is carried out under a protective gas atmosphere;

[0069] As a preferred embodiment, pre-carbonization helps the organic components inside the biomass material to carbonize and crack and overflow in the form of small molecular gases to form a stable framework structure. This structure can easily obtain a pore size distribution structure that is conducive to sodium storage during secondary high-temperature carbonization, thereby improving the electrochemical properties of the material.

[0070] Preferably, the protective gas includes any one or more of nitrogen, argon, helium or hydrogen.

[0071] (III) Removal of impurities:

[0072] The pre-carbonized biomass raw material is crushed into materials with a D50 particle size of 50 μm to 2 mm, dispersed at 30 to 60° C. for 0.5 to 12 hours, and then washed with deionized water for at least 5 times until it is neutral, to obtain a hard carbon precursor.

[0073] It should be noted that the above-mentioned neutral refers to a vague range concept of pH about 7 (6.5-7.5).

[0074] In a preferred embodiment of the present invention, the impurity removal is carried out by acid solution removal;

[0075] Preferably, the acid solution includes at least one of hydrochloric acid solution, sulfuric acid solution, nitric acid solution, oxalic acid, and citric acid solution;

[0076] As a preferred embodiment, the concentration of the acid solution is 0.1 to 5 mol / L;

[0077] In a preferred embodiment of the present invention, during the impurity removal process, the solid-to-liquid ratio of the pre-carbonized biomass raw material to the acid solution is 1:10-30;

[0078] (IV) Solid phase mixing:

[0079] The hard carbon precursor needs to be dried before being mixed with the ionic compound; the dried hard carbon precursor is further crushed and then mixed with the ionic compound in a solid phase;

[0080] In a preferred embodiment of the present invention, the crushed particle size D50 of the hard carbon precursor is 2 to 20 μm;

[0081] In a preferred embodiment of the present invention, the mass ratio of the hard carbon precursor to the ion-doped compound is 1:0.01-0.3, and the solid-phase mixing tool is one of a high-energy ball mill, a manual grinder or a mixer;

[0082] As a preferred implementation, the solid phase mixture can be mixed in different ways according to the characteristics of different ionic compounds. For example, metal ionic compounds that are easily absorbent can be mixed in a low-speed mixer or manually ground, while other materials can be mixed by high-energy spheroidal graphite.

[0083] In a preferred embodiment of the present invention, the ionic compound comprises a non-metallic compound and a metal ionic compound;

[0084] In the above preferred embodiment, the non-metallic compound includes at least one of urea, thiourea, ammonium chloride, melamine, and diammonium phosphate;

[0085] In the above preferred embodiment, the metal ion compound includes at least one of nitrates, phosphates and metal chlorides containing the metal elements manganese, zinc and iron.

[0086] (V) High temperature carbonization:

[0087] This is followed by high temperature carbonization treatment;

[0088] The pyrolysis temperature of the high-temperature carbonization treatment is 1000-1600° C., the pyrolysis treatment time is 2-6 hours, and the heating rate of the pyrolysis treatment is 1-5° C. / min.

[0089] According to one aspect of the present invention, a biomass hard carbon material is provided. The biomass hard carbon material is mainly prepared by the above-mentioned method for preparing the biomass hard carbon material.

[0090] According to one aspect of the present invention, the above-mentioned biomass hard carbon material is used in the preparation of a negative electrode plate for a sodium ion battery.

[0091] The biomass hard carbon material provided by the present invention can be widely used in the preparation process of the negative electrode sheet of a sodium ion battery.

[0092] According to one aspect of the present invention, a sodium ion battery negative electrode plate, the component raw materials of the sodium ion battery negative electrode plate, calculated by mass percentage, include:

[0093] Biomass hard carbon material 90-95%, conductive carbon black (SP) 1-5%, polyvinylidene fluoride (PVDF) 1-5%.

[0094] Preferably, the sodium ion battery negative electrode plate is prepared by the following steps:

[0095] The biomass hard carbon material, SP and PVDF are dissolved in NMP to prepare the battery negative electrode slurry; the battery negative electrode slurry is coated on the surface of the metal aluminum foil, and then dried to obtain the sodium ion battery negative electrode material.

[0096] According to one aspect of the present invention, a sodium ion battery comprises the above-mentioned sodium ion battery negative electrode sheet.

[0097] Preferably, the sodium ion battery further comprises a positive electrode plate, an electrolyte, and a diaphragm;

[0098] Preferably, the raw material of the positive electrode plate is one or a combination of at least two of layered oxides, Prussian blue compounds and polyanion compounds.

[0099] The technical solution of the present invention will be further described below in conjunction with embodiments.

[0100] Example 1

[0101] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0102] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0103] S2. Pre-carbonization: Take the dried walnut shell material and heat it to 600°C at 3°C / min under a nitrogen atmosphere and keep it warm for 3 hours to obtain a biomass pre-carbonized material;

[0104] S3, pickling: crush the pre-carbonized material into a material with a D50 particle size of 1 mm, then mix it with a 3 mol / L hydrochloric acid solution at a material-liquid ratio of 1:10, and then magnetically disperse it at 50°C for 3 hours, then wash it with deionized water and dry it for use;

[0105] S4, ion doping mixture: the pre-carbonized material after acid washing is further crushed into a D50 of 8 μm, and then it is added into a low-speed mixer with zinc chloride at a mass ratio of 1:0.05 and continuously dispersed at 70 rpm / min for 1 hour to obtain a precursor material;

[0106] S5. High temperature carbonization: The precursor material is heated to 1400° C. at a rate of 3° C. / min under a nitrogen atmosphere and then kept at this temperature for 3 hours to obtain the zinc ion-modified biomass hard carbon material.

[0107] Example 2

[0108] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0109] S1, pre-cleaning and drying: 100g of bamboo was dispersed in 1L of domestic water, and the mixture was removed after being dispersed and stirred. The pre-cleaning process was continued for 2 times, and then the mixture was dried in a blast drying oven for standby use;

[0110] S2. Pre-carbonization: Take the dried material and heat it to 400°C at 10°C / min in a nitrogen atmosphere and keep it warm for 4 hours to obtain the biomass pre-carbonized material;

[0111] S3, pickling: crush the pre-carbonized material into a material with a D50 particle size of 50 μm, then mix it with a 3 mol / L oxalic acid solution at a material-liquid ratio of 1:10, and then magnetically disperse it at 50°C for 3 hours, then wash it with deionized water and dry it for use;

[0112] S4, ion doping mixture: the pre-carbonized material after acid washing is further crushed into D50 of 3 μm, and then it is added into a low-speed mixer with manganese chloride at a mass ratio of 1:0.03 and dispersed at 70 rpm / min for 1 hour to obtain a precursor material;

[0113] S5. High temperature carbonization: heating the precursor material to 1300° C. at 2° C. / min under an argon atmosphere and then keeping the temperature for 3 hours to obtain the ion-modified biomass hard carbon material;

[0114] Example 3

[0115] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0116] S1, pre-cleaning and drying: take 100g of rice husk and disperse it in 1L of domestic water, stir and remove it, the pre-cleaning process is repeated twice, and then it is dried in a blast drying oven for later use;

[0117] S2. Pre-carbonization: Take the dried material and heat it to 400°C at 2°C / min in a nitrogen atmosphere and keep it warm for 3 hours to obtain the biomass pre-carbonized material;

[0118] S3, pickling: crush the pre-carbonized material into a material with a D50 particle size of 2 mm, then mix it with a 5 mol / L sulfuric acid solution at a material-liquid ratio of 1:30, and then magnetically disperse it at 50°C for 3 hours, then wash it with deionized water and dry it for use;

[0119] S4, ion doping mixture: the pre-carbonized material after pickling is further crushed into D50 of 10 μm, and then added into the spherical ink tank with manganese dihydrogen phosphate at a mass ratio of 1:0.01, and the mass ratio of the material balls is 1:10, and dispersed at a high speed of 500 rpm / min for 30 minutes to obtain the precursor material;

[0120] S5. High temperature carbonization: heating the precursor material to 1600° C. at 5° C. / min under an argon atmosphere and then keeping the temperature for 2 h to obtain the ion-modified biomass hard carbon material;

[0121] Example 4

[0122] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0123] S1. Pre-carbonization: Take 100 g of cellulose and heat it to 400°C at 3°C / min in a nitrogen atmosphere and keep it warm for 3 hours to obtain a biomass pre-carbonized material;

[0124] S2. Ion doping mixture: add the pre-carbonized material with a D50 of 2 μm and zinc nitrate in a mass ratio of 1:0.05 into a low-speed mixer and disperse at 70 rpm / min for 1 hour to obtain a precursor material;

[0125] S3. High temperature carbonization: The precursor material is heated to 1300° C. at a rate of 2° C. / min under a nitrogen atmosphere and then kept at this temperature for 3 hours to obtain the ion-modified biomass hard carbon material.

[0126] This embodiment is an implementation method of directly ion doping the cellulose precursor without acid washing to remove impurities.

[0127] Example 5

[0128] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0129] S1. Pre-carbonization: Take 100g of starch in a nitrogen atmosphere, heat it to 400℃ at 1℃ / min, and keep it warm for 6h to obtain biomass pre-carbonized material;

[0130] S2. Ion doping mixture: The pre-carbonized material after pickling is further crushed into a D50 of 20 μm, and then urea is added into the ball ink tank at a mass ratio of 1:0.1, and the mass ratio of the material balls is 1:10. The precursor material can be obtained by high-speed dispersion at a speed of 500 rpm / min for 30 minutes.

[0131] S3. High temperature carbonization: The precursor material is heated to 1000° C. at a rate of 1° C. / min under a nitrogen atmosphere and then kept at this temperature for 6 hours to obtain the ion-modified biomass hard carbon material.

[0132] This embodiment is an implementation method of directly ion doping the starch body without acid washing and impurity removal.

[0133] Example 6

[0134] In this embodiment, step S4 is as follows:

[0135] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into D50 of 10 μm, and then added into the spherical ink tank with ammonium chloride at a mass ratio of 1:0.3, and the mass ratio of the material balls is 1:10, and high-speed dispersion is carried out at a speed of 500 rpm / min for 30 minutes to obtain the precursor material”.

[0136] Example 7

[0137] In this embodiment, step S4 is as follows:

[0138] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into a D50 of 10 μm, and then added into a ball ink tank with melamine at a mass ratio of 1:0.1, and the mass ratio of the material balls is 1:10, and dispersed at a high speed of 500 rpm / min for 30 minutes to obtain the precursor material”.

[0139] Example 8

[0140] In this embodiment, step S4 is as follows:

[0141] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into D50 of 8 μm, and then added into the spherical ink tank with diammonium hydrogen phosphate at a mass ratio of 1:0.08, and the mass ratio of the material balls is 1:10, and high-speed dispersion is carried out at a speed of 500 rpm / min for 30 minutes to obtain the precursor material”.

[0142] Example 9

[0143] In this embodiment, step S4 is as follows:

[0144] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into a D50 of 8 μm, and then added into a low-speed mixer with manganese chloride at a mass ratio of 1:0.03 and continuously dispersed at 70 rpm / min for 1 hour to obtain a precursor material”.

[0145] Example 10

[0146] In this embodiment, step S4 is as follows:

[0147] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into D50 of 8 μm, and then added into the spherical ink tank with thiourea at a mass ratio of 1:0.2, and the mass ratio of the material balls is 1:10, and high-speed dispersion is carried out at a speed of 500 rpm / min for 30 minutes to obtain the precursor material”.

[0148] Embodiment 11

[0149] In this embodiment, step S4 is as follows:

[0150] The same as Example 1 except that “the pre-carbonized material after pickling is further crushed into D50 of 10 μm, and then added into the spherical ink tank with zinc phosphate at a mass ratio of 1:0.05, and the mass ratio of the material balls is 1:10, and high-speed dispersion is carried out at a speed of 500 rpm / min for 30 minutes to obtain the precursor material”.

[0151] Example 12

[0152] In this embodiment, step S4 is as follows:

[0153] The same as Example 1 except that “the pre-carbonized material after acid washing is further crushed into a D50 of 5 μm, and then it is added into a low-speed mixer with ferric chloride in a mass ratio of 1:0.03 and dispersed at 70 rpm / min for 1 hour to obtain a precursor material”.

[0154] Example 13

[0155] This embodiment is the same as Embodiment 1 except that in step S3, "3 mol / L hydrochloric acid solution" is replaced by "0.5 mol / L hydrochloric acid solution".

[0156] Embodiment 14

[0157] This embodiment is the same as Embodiment 1 except that in step S3, "3 mol / L hydrochloric acid solution" is replaced by "0.1 mol / L hydrochloric acid solution".

[0158] Embodiment 15

[0159] This embodiment is the same as Embodiment 1 except that in step S3, "3 mol / L hydrochloric acid solution" is replaced by "3 mol / L citric acid solution".

[0160] Example 16

[0161] This embodiment is the same as Embodiment 1 except that in step S3 the pre-carbonized material is crushed into material with a D50 particle size of 5 mm.

[0162] Embodiment 17

[0163] This embodiment is the same as Embodiment 1 except that in step S3, "the pre-carbonized material is mixed with 3 mol / L hydrochloric acid solution at a material-liquid ratio of 1:8".

[0164] Embodiment 18

[0165] This embodiment is the same as Embodiment 1 except that in step S3, "the pre-carbonized material is mixed with 3 mol / L hydrochloric acid solution at a material-liquid ratio of 1:35".

[0166] Embodiment 19

[0167] This embodiment is the same as Embodiment 1 except that in step S4, "pre-carbonized material with a D50 of 35 μm after pickling" is mixed with zinc chloride in a low-speed mixer.

[0168] Embodiment 20

[0169] This embodiment is the same as Embodiment 1 except that in step S4, "pre-carbonized material with a D50 of 1 μm after pickling" is mixed with zinc chloride in a low-speed mixer.

[0170] Embodiment 21

[0171] This embodiment is the same as Embodiment 1 except that in step S4, "the pre-carbonized material with a D50 of 8 μm after pickling and zinc chloride are added into the spherical ink tank at a mass ratio of 1:0.05, the mass ratio of the material balls is 1:10, and they are dispersed at a high speed of 500 rpm / min for 30 min."

[0172] Embodiment 22

[0173] This embodiment is the same as Embodiment 1 except that in step S4, "pre-carbonized material with a D50 of 3 μm after pickling" is mixed with zinc chloride in a low-speed mixer.

[0174] Embodiments 23 to 28

[0175] This embodiment is the same as that in Embodiment 1 except that the process parameters of high temperature carbonization in step S5 are different from those in Embodiment 1.

[0176] The process parameters of high temperature carbonization of Examples 23 to 28 are shown in Table 1:

[0177] Table 1:

[0178]

[0179] Comparative Example 1

[0180] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0181] S1. High temperature carbonization: The biomass walnut shell material is heated to 1200° C. at 5° C. / min in a nitrogen atmosphere and then kept at this temperature for 2 hours to obtain the biomass hard carbon material.

[0182] Comparative Example 2

[0183] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0184] S1. Pre-cleaning and drying:

[0185] Take 100g of walnut shell waste and disperse it in 1L of domestic water, then take it out after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then it is dried in a blast drying oven for use;

[0186] S2. High temperature carbonization:

[0187] The precursor material is heated to 1200° C. at a rate of 5° C. / min under a nitrogen atmosphere and then kept at this temperature for 2 hours to obtain the biomass hard carbon material.

[0188] Comparative Example 3

[0189] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0190] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0191] S2. Pre-carbonization: Take the dried walnut shell material and heat it to 600°C at 3°C / min under a nitrogen atmosphere and keep it warm for 3 hours to obtain a biomass pre-carbonized material;

[0192] S3, pickling: crush the pre-carbonized material into a material with a D50 particle size of 1 mm, then mix it with a 3 mol / L hydrochloric acid solution at a material-liquid ratio of 1:10, and then magnetically disperse it at 50°C for 3 hours, then wash it with deionized water and dry it for use;

[0193] S4. High-temperature carbonization: The acid-washed precursor material is heated to 1400° C. at a rate of 3° C. / min in a nitrogen atmosphere and then kept at this temperature for 3 hours to obtain the ion-modified biomass hard carbon material.

[0194] This embodiment is the same as Embodiment 1 except that it does not include the ion doping mixing step.

[0195] Comparative Example 4

[0196] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0197] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0198] S2. Ion doping mixing: The dried walnut shell material was crushed into a material with a D50 particle size of 1 mm, and then added with zinc chloride in a mass ratio of 1:0.1 into a low-speed mixer and dispersed at 70 rpm / min for 1 hour;

[0199] S3, pre-carbonization: the mixed material is heated to 600°C at 3°C / min under a nitrogen atmosphere and then kept at this temperature for 3 hours to obtain a carbon precursor;

[0200] S4, high temperature carbonization: the precursor material is heated to 1200°C at 5°C / min under a nitrogen atmosphere and then kept at this temperature for 2 hours to obtain the zinc ion-modified biomass hard carbon material;

[0201] Comparative Example 5

[0202] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0203] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0204] S2. Ion doping mixing: The biomass raw material was crushed into a D50 of 8 μm, and then added into a low-speed mixer with zinc chloride at a mass ratio of 1:0.1 and continuously dispersed at 70 rpm / min for 1 hour;

[0205] S3, high temperature carbonization: the precursor material is heated to 1200°C at 5°C / min in a nitrogen atmosphere and then kept at this temperature for 2 hours to obtain the zinc ion-modified biomass hard carbon material;

[0206] Comparative Example 6

[0207] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0208] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0209] S2, pickling: crush the pre-carbonized material into a material with a D50 particle size of 1 mm, then mix it with a 3 mol / L hydrochloric acid solution at a material-liquid ratio of 1:10, and then magnetically disperse it at 50°C for 3 hours, then wash it with deionized water and dry it for use;

[0210] S3, ion doping mixture: the pre-carbonized material after acid washing is further crushed into D50 of 8 μm, and then mixed in a 0.05 mol / L manganese chloride aqueous solution with a solid-liquid ratio of 1:10, and after magnetic dispersion for 2 hours, filtered and dried to obtain the precursor material;

[0211] S4, high temperature carbonization: the precursor material is heated to 1200°C at 5°C / min under a nitrogen atmosphere and then kept at this temperature for 2 hours to obtain the zinc ion-modified biomass hard carbon material;

[0212] Comparative Example 7

[0213] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0214] S1, pre-cleaning and drying: take 100g of walnut shell waste and disperse it in 1L of domestic water, remove it after dispersion and stirring, and the pre-cleaning process is continued for 2 times, and then dried in a blast drying oven for standby use;

[0215] S2. Pre-carbonization: Take the dried walnut shell material and heat it to 600°C at 3°C / min under a nitrogen atmosphere and keep it warm for 3 hours to obtain a biomass pre-carbonized material;

[0216] S3, ion doping mixing: the pre-carbonized material is further crushed into a D50 of 8 μm, and then mixed with zinc chloride in a mixer at a mass ratio of 1:0.05 to obtain a precursor material;

[0217] S4. High temperature carbonization: The precursor material is heated to 1400° C. at a rate of 3° C. / min under a nitrogen atmosphere and then kept at this temperature for 3 hours to obtain the ion-modified biomass hard carbon material.

[0218] This embodiment is the same as Embodiment 1 except that it does not include the pickling and impurity removal step.

[0219] Comparative Examples 8 to 13

[0220] This embodiment is the same as Embodiment 1 except that the process parameters of the pre-carbonization treatment in step S2 are different from those in Embodiment 1.

[0221] The process parameters of the pre-carbonization treatment of Comparative Examples 8 to 13 are shown in Table 2:

[0222] Table 2:

[0223]

[0224] Comparative Example 14

[0225] This embodiment is the same as the first embodiment except step S4 "the mass ratio of the acid-washed hard carbon precursor material to zinc chloride is 1:0.008".

[0226] Comparative Example 15

[0227] This embodiment is the same as the first embodiment except step S4 "the acid-washed hard carbon precursor material and zinc chloride are mixed in a mass ratio of 1:0.35".

[0228] Comparative Example 16

[0229] This embodiment is the same as the embodiment 1 except step S4 "the hard carbon precursor material after acid washing is dispersed in a 0.1 mol / L zinc chloride aqueous solution with a solid-liquid ratio of 1:20, and after dispersion for 6 hours, it is filtered and dried for later use".

[0230] Comparative Example 17

[0231] A method for preparing a biomass hard carbon material, the preparation method comprising:

[0232] S1, pre-cleaning and drying: same as in Example 1;

[0233] S2, pre-carbonization: same as in Example 1;

[0234] S3, ion doping mixture: the pre-carbonized material is further crushed into a D50 of 8 μm, and then it is added to a low-speed mixer with zinc chloride at a mass ratio of 1:0.05 and dispersed at 70 rpm / min for 1 hour to obtain a precursor material;

[0235] S4. High-temperature carbonization: The precursor material is heated to 1400°C at 3°C / min under a nitrogen atmosphere and then kept warm for 3 hours. After natural cooling, it is immersed in an acidic solution and then washed with deionized water and ethanol until neutral. The obtained product is placed in a vacuum drying oven and vacuum dried to obtain the zinc ion-modified biomass hard carbon material.

[0236] The acid solution is a 3 mol / L hydrochloric acid solution, and the soaking time is 6 hours; the temperature of the vacuum drying oven is 80° C., and the drying time is 12 hours.

[0237] The difference between this comparative example and Example 1 is that: the step of acid washing the pre-carbonized material is not included before the ion doping mixture, and this comparative example also includes the steps of soaking the product material in an acid solution and drying it after high-temperature carbonization.

[0238] Test Example 1

[0239] In order to demonstrate the performance of the biomass hard carbon material prepared in the present application, the following electrochemical performance test is now carried out.

[0240] (I) Test sample preparation:

[0241] 1. The metal ion-modified biomass hard carbon materials provided in Examples 1 to 28, and the modified biomass hard carbon materials provided in Comparative Examples 1 to 16;

[0242] 2. Preparation of sodium ion batteries using the above biomass hard carbon materials:

[0243] Preparation of negative electrode sheets for sodium ion batteries: 95 parts of hard carbon negative electrode materials, 3 parts of SuperP, and 2 parts of binder (specific name: PVDF) are weighed by mass, and dissolved in NMP to obtain battery negative electrode slurry; the battery negative electrode slurry is applied on the surface of aluminum foil with a coating amount of 4 mg / cm2, and vacuum dried in a vacuum drying oven at 100°C for 10 hours, and the electrode sheets are cut with a mold to obtain the sodium ion battery negative electrode sheets.

[0244] Assembly of sodium-ion battery: Sodium metal was used as the counter electrode, the electrolyte was 1 mol / L NaPF6 (the solvent was DEGDME), and the separator was glass fiber (GF / A), and a C2032 button cell was formed in a glove box filled with argon.

[0245] (II) Performance testing:

[0246] 1. Charge and discharge performance test: The test was conducted using the CT-4008 battery test system of Wuhan Landian Electronics Co., Ltd. The test results are shown in Tables 3 to 8.

[0247] Figure 1 The first charge and discharge curves of Example 1, Example 6 and Comparative Example 3 provided in this test example.

[0248] Figure 2 The cycle performance diagrams of Example 1, Example 6, and Comparative Example 3 provided in this test example at a 1C rate.

[0249] 2. XRD test method:

[0250] By using a light source with a known wavelength of λ as the excitation source, measuring the angle with an X-ray spectrometer, and calculating the d value of the crystal that produces diffraction, the lattice spacing of the analyzed substance can be known, thereby understanding the structural properties of the object to be tested. The 2θ test range is 10° to 80°, and the step length is 0.2-0.3 of FWHM. See Tables 3 to 8 for specific test results.

[0251] Figure 3 X-ray diffraction patterns of Example 1, Example 6, and Comparative Example 3 provided for this test example.

[0252] It should be noted that the units of the performance test items in the following Tables 3 to 8 are as follows: charging capacity (mAh / g), discharge capacity (mAh / g), first-week coulombic efficiency (%), 1C rate capacity (mAh / g), cycle capacity retention rate (1C / 200 cycles, %), and d002 (nm).

[0253] Table 3:

[0254]

[0255] Table 4:

[0256]

[0257]

[0258] Table 5:

[0259]

[0260] Table 6:

[0261]

[0262]

[0263] Table 7:

[0264]

[0265] Table 8:

[0266]

[0267]

[0268] It can be seen from the electrochemical performance test results in Tables 3 to 8 above that the ion-doped modified biomass hard carbon materials prepared by the solid phase method in Examples 1 to 15 of the present application have excellent electrochemical properties, and the gram capacity, first efficiency and cycle performance are greatly improved. Among them, Example 1 has the best ion doping effect, with a reversible gram capacity of up to 326mah / g and a first efficiency of >90%.

[0269] The processing experimental parameters of Examples 16 to 28 of the present application are beyond the experimental parameter range of the present application. It can be found that the electrochemical performance is significantly deteriorated compared with Examples 1 to 15, indicating that each process treatment step works synergistically on the ion doping effect to make the structure of the hard carbon material controllable, and the electrochemical performance can be significantly improved. A single experimental parameter beyond the controllable range will greatly affect the material structure characteristics and deteriorate the electrochemical performance.

[0270] At the same time, it can be seen from the experimental data in the above table that in the process of carbonization treatment by the solid phase method of the present application: non-metallic compounds adjust the material properties through chemical bonding between N and S atoms and C atoms of hard carbon in the high-temperature carbonization stage, optimize the carbon layer information, grain size and improve the conductivity of the material through chemical bonding, thereby improving the reversibility of sodium ion deintercalation; metal compounds adjust the biomass hard carbon structure more by catalytic modification of metal ions, and generate pores in the form of small molecules overflowed by ionic compounds in the middle stage of carbonization. In the later stage of carbonization, closed pores suitable for sodium ion deintercalation are formed through the growth and repair of carbon material grains. More sodium storage sites are created mainly through the regulation of the hard carbon structure, thereby improving the electrochemical properties of biomass hard carbon; both methods belong to the regulation of the microstructure of carbon materials, and the macrostructure remains unchanged.

[0271] Further, referring to Tables 3 to 8, we can see that:

[0272] Example 1 is an implementation method of ion doping after acid washing of walnut shell precursor; Example 4 is an implementation method of direct ion doping of cellulose precursor without acid washing and impurity removal; Example 5 is an implementation method of direct ion doping of starch precursor without acid washing and impurity removal, all of which show excellent electrochemical performance. This shows that acid washing can improve the doping effect of biomass hard carbon containing impurities and reduce the influence of impurity elements on the ion doping effect; high-purity biomass raw materials can also achieve good ion doping effects without acid washing, indicating that ion doping is applicable to the existing broad biomass material system and is a universal performance improvement method;

[0273] Compared with Examples 1 to 15, the material after pre-carbonization in Example 16 was crushed to a D50 particle size that exceeded the experimental parameter range of 50 μm to 2 mm, and the electrochemical performance was significantly degraded. This is because the material with a crushed particle size greater than 2 mm will cause incomplete pickling and impurity removal of the pre-carbonized material after the pickling process, and some impurity elements will affect the subsequent ion doping effect and reduce the electrochemical performance. The material below 50 μm will reduce the efficiency of pickling and impurity removal, wasting energy consumption;

[0274] Compared with Examples 1 to 15, the solid-liquid ratio of the acid pickling section precursor to the acid solution in Examples 17 to 18 exceeds the experimental parameter range of 1:10 to 30, and the electrochemical performance deteriorates significantly. This is because the low-concentration acid impurity removal effect is poor, and the presence of a large number of impurity elements inhibits the ion doping effect; the high-concentration acid impurity removal process will destroy the carbon structure framework, and the high-temperature section cannot be repaired; both will cause significant degradation of the electrochemical performance;

[0275] Compared with Examples 1 to 15, the particle size D50 of the impurity-removing precursor in the solid phase mixing process of Examples 19 to 20 exceeds the experimental parameter range of 2 to 20 μm, and the electrochemical performance deteriorates significantly. This is because the hard carbon precursor with a small particle size is conducive to improving the uniformity of ion doping, ensuring that the ionic compounds can uniformly adhere to the surface of the precursor and penetrate into the interior, thereby regulating the hard carbon structure. Larger particles outside the parameter range will cause non-uniform ion doping and fail to penetrate into the interior of the precursor normally, and have little effect on regulating the hard carbon structure; particles outside the parameter range are too small, which will cause the specific surface area of ​​the precursor material to increase, affecting the penetration efficiency of ion doping. At the same time, the hard carbon material obtained will also cause irreversible deintercalation of sodium ions due to the large specific surface area, and the first effect will be greatly reduced.

[0276] Compared with Examples 1 to 15, Examples 21 to 22 did not select the correct mixing method according to the characteristics of the ionic compounds during the solid phase mixing process, and the electrochemical performance deteriorated significantly. This is because the hard carbon precursor in the high-energy ball milling mixing of the easily water-absorbing metal ionic compounds agglomerated and adhered to the inside of the ball ink tank, resulting in uneven mixing and affecting the doping effect; other ionic compounds were mixed by a mixer at a low speed or manually ground, which reduced the doping effect due to uneven mixing;

[0277] Compared with Examples 1 to 15, the process parameters (temperature, time, heating rate) of high-temperature carbonization in Examples 23 to 28 exceeded the carbonization parameter range of Examples 1 to 15, and the electrochemical performance deteriorated significantly. This is because ion doping needs to stably achieve the effect of ion doping under appropriate carbonization conditions, which has a positive effect on the electrochemical performance. Carbonization conditions outside the range have a weak effect on the performance gain of hard carbon, and even deteriorate the performance. Ion doping and high-temperature carbonization are synergistic effects.

[0278] Furthermore, referring to Tables 3 to 8, it can be seen that in Example 1, the raw materials are directly subjected to high-temperature carbonization treatment, Example 2 is a solution in which the raw materials are pre-cleaned and dried and then directly subjected to high-temperature carbonization treatment, and Example 3 is a solution in which the raw materials are pre-cleaned, pre-carbonized and then subjected to high-temperature carbonization (excluding the ion doping mixing step).

[0279] Comparative Examples 1 and 2 show that pre-cleaning can remove impurities such as ash, stone, and soil on the surface of the raw materials that cannot be carbonized, thereby reducing the degradation of the hard carbon performance. Pre-cleaning can significantly improve the electrochemical performance, thereby indicating the necessity of the pre-cleaning effect.

[0280] Comparative Example 2 and Comparative Example 3 show that pre-carbonization forms a stable framework for the carbon layer and adjusts the pores by adjusting the structure of the precursor. It also allows sufficient reaction time for high-temperature carbonization of hard carbon to obtain a structurally stable material, thereby improving the electrochemical properties of the material. However, it is significantly inferior to the electrochemical properties of the solid-phase doping of Examples 1 to 15.

[0281] Comparative Example 4 is a scheme in which the raw materials and ionic compounds are doped and mixed before pre-carbonization treatment, followed by impurity removal treatment, and finally high-temperature carbonization. Compared with Example 1, the electrochemical performance is seriously degraded. This is because low-temperature ion doping will be affected by the cracking and overflow of organic components in the biomass raw materials during the pre-carbonization process, causing some doped ions to react with the cracking gas and damage the biomass hard carbon, resulting in poor ion doping effect in the high-temperature carbonization stage;

[0282] Comparative Example 5 is a solution in which the raw materials are doped with ionic compounds and then directly carbonized at high temperature. Compared with Example 1, the electrochemical performance is seriously deteriorated, indicating that during the carbonization process of the biomass raw materials, due to the cracking of the internal organic components and the presence of impurities (insoluble and soluble), the ion doping causes irreversible damage to the hard carbon structure in the high-temperature carbonization stage, resulting in performance degradation;

[0283] Comparative Example 6 is a scheme that does not include the pre-carbonization treatment in Example 1 (other treatment methods are the same). Compared with Example 1, the electrochemical performance is seriously deteriorated. This is because the one-step carbonization of biomass hard carbon will cause defects in the low-temperature framework, and there is not enough carbonization time for repair in the high-temperature section, resulting in many material defects; at the same time, ionic compounds will react with small gas molecules in the low-temperature section and overflow, which will aggravate the increase of defects, thereby significantly deteriorating the electrochemical performance;

[0284] Comparative Example 7 is a scheme that does not include the pickling and impurity removal step in Example 1 (other treatment methods are the same). Compared with Example 1, the electrochemical performance is seriously deteriorated. This is because the ion doping modification improves the electrochemical performance of the unmodified hard carbon by improving the conductivity, adjusting the carbon layer spacing, adjusting the pore structure information, etc., but due to the influence of the impurity elements inside the raw materials, part of the ion doping effect will be inhibited. By adding the pickling and impurity removal, the drying of the impurity elements on the doping effect is further reduced, and the electrochemical performance can be further optimized;

[0285] Comparative Examples 8 to 13 are schemes in which the process parameters of the pre-carbonization treatment are not within the scope of the embodiments of the present application (other treatment methods are consistent). Compared with Example 1, the electrochemical performance is seriously degraded. This is because the carbon structure framework is controllably regulated by adjusting the pre-carbonization parameters, but appropriate pre-carbonization parameters are required. Pre-carbonization parameters outside the range will cause the collapse of the carbon framework structure or greatly increase the carbon structure defects. In this case, the ion doping modification performance is seriously degraded, indicating that ion doping requires a stable carbon framework structure;

[0286] In particular, the pre-carbonization treatment temperature of Comparative Examples 8 and 9 is not within the range of 400 to 800°C of the present application. In Comparative Example 8, the pre-carbonization treatment temperature is 350°C, and its charging capacity is only 266mAh / g, and the electrochemical performance is seriously degraded. This is because the organic components inside the raw material will decompose into gas before 400°C to overflow and form a carbon layer framework. At 350°C, the organic components inside the raw material cannot be completely decomposed. In the later high-temperature carbonization process, the residual organic components continue to decompose, destroying the carbon layer framework, and the carbon structure collapses, but the base hard carbon is unstable, resulting in poor zinc ion doping effect; Comparative Example 9 has a pre-carbonization treatment temperature of 850°C, and its electrochemical performance is also poor. This is because excessive pre-carbonization temperature will cause carbon microcrystals to grow and thicken the carbon layer framework. During the high-temperature carbonization process, some zinc ions cannot penetrate into the hard carbon to form closed micropores through sublimation, thereby reducing the closed-pore sodium storage effect of the hard carbon, so the electrochemical performance is poor. This fully demonstrates that the selection of the pre-carbonization treatment temperature in the present application has a significant impact on the performance of the biomass hard carbon material finally prepared. Only the implementation method within the range of 400 to 800°C in the present application can achieve the effect of obtaining high-capacity and first-effect biomass hard carbon materials.

[0287] Comparative Examples 14 and 15 are schemes in which the mass ratio of the hard carbon precursor material to zinc chloride after pickling is not within the scope of the embodiments of the present application (other treatment methods are consistent). Compared with Example 1, the electrochemical performance is seriously deteriorated. This is because the effect of low-concentration zinc ion doping is not obvious, resulting in a low degree of improvement in the electrochemical performance, which is mainly reflected in the increase in the first effect; high-concentration zinc ion doping will increase the zinc ion content inside the hard carbon due to the increase in the doping amount, and excessively high zinc ion content will cause a large increase in hard carbon defects, the escape of sodium ions will be inhibited, the reversible capacity will be reduced, and the first effect will be greatly reduced.

[0288] Comparative Example 16 is a solution of liquid phase doping modification (other treatment methods are the same). Compared with Example 1, the electrochemical performance is seriously deteriorated. This is because the ion doping efficiency of liquid phase doping is low, and the amount of ion doping cannot be accurately controlled. The content of doped ions embedded in the hard carbon during the liquid phase doping process is small. With the overflow of ions during the high-temperature carbonization process, the amount of modified ions for hard carbon is further reduced, resulting in an insignificant ion doping effect. Solid phase doping can achieve controllable ion doping by regulating the mass ratio of ionic compounds to precursors, and achieve controllable modification of biomass hard carbon with sufficient ions, thereby obtaining biomass hard carbon materials with excellent electrochemical properties. The biomass hard carbon doped with liquid phase ions is obviously not as good as the effect of solid phase doping. Solid-phase doping achieves the adjustment of hard carbon structure by physically combining hard carbon and ionic compounds and decomposing ionic compounds during high-temperature carbonization. The amount of ion doping in solid-phase doping is controllable, avoiding the inaccuracy of liquid-phase ion doping. Solid-phase doping also reduces the use of ionic compounds, while improving the production efficiency of ion doping, reducing energy consumption and doping costs. It can effectively avoid the large amount of waste liquid pollution caused by the liquid-phase doping process, save processes and labor, and is more suitable for large-scale production of materials.

[0289] Comparative Example 17 is a scheme that does not include the step of pickling the pre-carbonized material before ion doping the mixture, and the steps of soaking the product material after high-temperature carbonization in an acid solution and drying it. Compared with Example 1, the electrochemical performance is seriously deteriorated. This is because, on the one hand, the impurity elements inside the raw materials will react with the ionic compounds to degrade the ion doping effect, and on the other hand, the finished product will expose many surface defects through pickling and impurity removal, increase the specific surface area of ​​the material, increase the irreversible sodium storage consumption, and reduce the first effect. The combined effect of these two aspects causes the electrochemical performance to deteriorate significantly.

[0290] Test Example 2

[0291] In order to demonstrate the physical and chemical index information of the biomass hard carbon material prepared in the present application, the following electrochemical evaluation test is now carried out.

[0292] Test samples:

[0293] The metal ion-modified biomass hard carbon materials provided in Example 1, Example 6 and Comparative Example 1;

[0294] 1. SEM characterization test method:

[0295] Through the interaction between the light beam and the material, various physical information is stimulated, and this information is collected, amplified, and re-imaged to achieve the purpose of characterizing the microscopic morphology of the material. The magnification of the collection is: 5000x, 10000x, 20000x. The test results are as follows Figures 4 to 6 shown.

[0296] Figure 4The scanning electron microscope image of Example 1 provided for this Experimental Example 2;

[0297] Figure 5 The scanning electron microscope image of Example 6 provided for this Experimental Example 2;

[0298] Figure 6 This is a scanning electron microscope image of Comparative Example 3 provided for this Experimental Example 2.

[0299] 2.TG test method:

[0300] Through the physical and chemical changes of the sample in the high temperature process, the weight changes with temperature / time during the program temperature process are recorded. The heating rate is 10℃ / min and the temperature is raised to 1400℃. The test results are as follows Figure 1 shown.

[0301] Figure 7 Thermogravimetric curves of the ionic compounds (zinc chloride, ammonium chloride, melamine) used in Example 1, Example 6, and Comparative Example 3 provided in this Experimental Example 2;

[0302] 3. Powder resistivity test method:

[0303] The resistance value is measured by applying a pressure to the sample to aggregate the powder together, which is used to evaluate the conductive properties of the material. The applied pressure is 20 MPa. The test results are shown in Table 4.

[0304] Table 9:

[0305]

[0306] It can be seen from Table 9 above that zinc ion and N element doping can significantly improve the conductivity of hard carbon, thereby improving the utilization rate of active materials to achieve the effect of optimizing electrochemical performance.

[0307] Based on the above test examples 1 and 2 Figure 1 to Figure 7 It can be seen that compared with the scheme of Comparative Example 3 (which does not include the ion doping mixing step), Example 1 and Example 6 achieve further increase in the carbon layer spacing by adjusting the framework structure of the hard carbon. At the same time, ion doping will not change the morphology of the hard carbon. It only achieves the sodium storage capacity of the pore structure by adjusting the pore size distribution inside the hard carbon. The biomass-modified hard carbon with excellent electrochemical properties is obtained through the combined regulation of the carbon layer spacing and the pore structure.

[0308] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a biomass hard carbon material, characterized in that: The preparation method comprises: The biomass raw material is pre-carbonized and then impurities are removed to obtain a hard carbon precursor; the hard carbon precursor is then mixed with an ionic compound using a solid phase method, and the solid phase mixed material is subjected to a high temperature carbonization treatment to obtain a biomass hard carbon material; The temperature of the pre-carbonization treatment is 400-800°C, the holding time is 2-6h, and the heating rate is 2-10°C / min; In the solid phase mixing process, the mass ratio of the hard carbon precursor to the ionic compound is 1:0.01-0.3; During the solid phase mixing process, the particle size D50 of the hard carbon precursor is 2 to 20 μm.

2. The method for preparing biomass hard carbon material according to claim 1, characterized in that: The biomass raw material comprises at least one of peanut shells, bamboo, walnut shells, coconut shells, almond shells, waste wood, rice husks and wheat husks; And / or, the biomass raw material includes at least one of glucose, starch, cellulose and lignin.

3. The method for preparing biomass hard carbon material according to claim 1, characterized in that: The pre-carbonization treatment is carried out under a protective gas atmosphere; Preferably, the protective gas includes any one or more of nitrogen, argon, helium or hydrogen.

4. The method for preparing biomass hard carbon material according to claim 1, characterized in that: The impurity removal is carried out by using an acid solution; Preferably, the acid solution includes at least one of hydrochloric acid solution, sulfuric acid solution, nitric acid solution, oxalic acid, and citric acid solution; More preferably, the acid solution has a concentration of 0.1 to 5 mol / L; Preferably, during the impurity removal process, the solid-to-liquid ratio of the pre-carbonized biomass raw material to the acid solution is 1:10-30; Preferably, the impurity removal method comprises: mixing the pre-carbonized biomass raw material and the acid solution and dispersing them at 30-60° C. for 0.5-12 hours, and then washing them with deionized water for at least 5 times until they are neutral, to obtain a hard carbon precursor; Preferably, the step of crushing the pre-carbonized biomass raw material is further included before the impurity removal, and the D50 of the crushed material is 50 μm to 2 mm.

5. The method for preparing biomass hard carbon material according to claim 1, characterized in that: The ionic compounds include non-metallic compounds and metal ionic compounds; Preferably, the non-metallic compound includes at least one of urea, thiourea, ammonium chloride, melamine, and diammonium phosphate; Preferably, the metal ion compound includes at least one of nitrates, phosphates and metal chlorides containing manganese, zinc and iron elements.

6. The method for preparing biomass hard carbon material according to claim 1, characterized in that: The pyrolysis temperature of the high-temperature carbonization treatment is 1000-1600° C., the pyrolysis treatment time is 2-6 hours, and the heating rate of the pyrolysis treatment is 1-5° C. / min.

7. A biomass hard carbon material, characterized in that: The biomass hard carbon material is mainly prepared by the preparation method of the biomass hard carbon material according to any one of claims 1 to 6.

8. Use of the biomass hard carbon material according to claim 7 in preparing negative electrode sheets for sodium ion batteries.

9. A negative electrode plate for a sodium ion battery, characterized in that: Measured by mass percentage, the component raw materials of the negative electrode plate of the sodium ion battery include: 90-95% of the biomass hard carbon material as described in claim 7, 1-5% of conductive carbon black, and 1-5% of polyvinylidene fluoride.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the sodium ion battery negative electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Element-doped biomass hard carbon negative electrode material for sodium-ion battery, preparation method and sodium-ion battery

    CN110571432A

  • Biomass hard carbon negative electrode material of sodium ion battery and preparation method of biomass hard carbon negative electrode material

    CN113206246A

  • Preparation and application of high-performance sodium-ion battery energy storage material based on regulation and control of hard carbon structure through ion catalysis

    CN114497543A

  • Novel biomass hard carbon sodium-ion battery material and preparation method thereof

    CN115353090A

  • Nitrogen and phosphorus co-doped sodium ion battery hard carbon negative electrode material and preparation method thereof

    CN116534839A

Cited By

  • Multi-stage pickling impurity removal method of coal-based hard carbon precursor for sodium storage

    CN119160877A

  • Preparation method of new substance derived hard carbon negative electrode material

    CN120793885A

  • Preparation method of biomass carbonized material with low silicon and aluminum content

    CN121405069A