Preparation method of barium titanate powder
Through the method of adding PVP in two steps and the hydrothermal reaction under alkaline conditions, the problems of powder agglomeration and uneven particle size distribution in the preparation of barium titanate powder were solved, and the preparation of barium titanate powder with good dispersion was achieved. , meets the raw material requirements of high-end ceramic capacitors and is suitable for industrial production.
Patent Information
- Application Number
- CN202410999330.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing barium titanate powder preparation methods, there are problems such as easy agglomeration of powders, excessive grain growth and uneven particle size distribution, and the low production efficiency of hydrothermal method is not conducive to industrial production.
The method of adding polyvinylpyrrolidone (PVP) is adopted. First, mix the barium source and titanium source under alkaline conditions, and then heat up and react with the remaining PVP to control the concentration and addition method of PVP to prevent powder agglomeration and eliminate it by calcination. The surface hydroxyl group increases the proportion of four-sided phase.
Barium titanate powder with narrow particle size distribution and good dispersion is obtained, which meets the raw material requirements of high-end MLCC products. It has a simple process and a wide range of applications. It is suitable for large-scale industrial production.
Smart Images

Figure BDA0004961122190000061 
Figure BDA0004961122190000071 
Figure BDA0004961122190000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ceramic materials, and in particular relates to a method for preparing barium titanate powder. Background Art
[0002] In recent years, the development of MLCC (multilayer ceramic capacitor) technology has mainly focused on high capacity, high voltage, base metal, miniaturization and multifunctionality of products. The above development directions can be fundamentally attributed to increasing capacity and reducing costs. At present, the technical approach to increasing the capacity of ceramic capacitor products focuses on improving the performance of ceramic materials and developing new material systems, improving the dielectric constant of ceramic materials, reducing the thickness of the dielectric layer and increasing the number of stacking layers. Barium titanate powder, as the main crystal material, is a key factor affecting the performance of MLCC. In order to adapt to the development of miniaturization and high stability of electronic devices, the technology puts forward high-purity and ultra-fine, or even higher requirements for barium titanate powder.
[0003] The main methods for industrial preparation of barium titanate powder are solid phase method and liquid phase method. The barium titanate prepared by the traditional solid phase method has more impurities, and the particle size is mostly micron or submicron, and the particle size distribution range is wide, which is only suitable for some electronic devices with relatively low technical performance requirements. The hydrothermal method adapts to the requirements of material development. By adjusting the reaction temperature, the concentration and type of mineralizer, the molar ratio of barium to titanium, the dispersant and other influencing factors, high-purity barium titanate with regular morphology, narrow particle size distribution range and small size is obtained. The hydrothermal method is currently divided into two methods: high temperature and high pressure hydrothermal method and atmospheric pressure hydrothermal method. The preparation conditions of high temperature and high pressure hydrothermal method are harsh, the reaction time is long, and the production efficiency is low, which is not conducive to industrial production. Although the atmospheric pressure hydrothermal method has a simple preparation environment and high production efficiency, the synthesized nano barium titanate powder has problems such as high proportion of cubic phase, easy aggregation of particles, and many surface hydroxyl defects. Although subsequent calcination can eliminate the surface hydroxyl groups of the powder and increase the proportion of tetragonal phase, high temperature will cause the nano powder to re-agglomerate and the particles to grow abnormally. Therefore, the research on the preparation of barium titanate nano powder by hydrothermal method still needs to be improved. Summary of the invention
[0004] In order to overcome the problems existing in the prior art, one of the objectives of the present invention is to provide a method for preparing barium titanate powder.
[0005] A second object of the present invention is to provide a multilayer ceramic capacitor.
[0006] A third object of the present invention is to provide a method for preparing the above-mentioned barium titanate powder and / or the application of the barium titanate powder prepared by the above-mentioned preparation method in ceramic products.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides a method for preparing barium titanate powder, comprising the following steps:
[0009] S1: mixing the barium source solution, part of the polyvinyl pyrrolidone solution, and the titanium source solution to obtain a mixed solution;
[0010] S2: adjusting the pH of the mixed solution to make the pH>12;
[0011] S3: heating, then mixing with the remaining polyvinyl pyrrolidone solution for reaction, and collecting the solid;
[0012] S4: calcining the solid to obtain the barium titanate powder.
[0013] In the present invention, polyvinyl pyrrolidone (PVP) is added in two steps, step S1 and step S3, respectively. The role of adding PVP in step S1 is mainly to disperse, prevent the barium source and the titanium source from reacting during the heating process of step S3, thereby causing the powder generated by the reaction to agglomerate and abnormal growth of the grains. At the same time, if the temperature has not reached the set temperature and all the PVP is added before the reaction begins, the amount of PVP in the reaction system will be too much, and the PVP itself will undergo a cross-linking reaction to produce gel micelles, which will affect the dispersibility of the barium titanate powder (i.e., BT powder). Therefore, in step S3, the present invention heats up to allow the temperature to reach the set temperature before adding the remaining PVP. If PVP is added to the reaction system at one time, the PVP content in the reaction system will be too high. As the reaction temperature increases, PVP itself is prone to cross-linking reactions, producing gel micelles, and the viscosity of the reaction system will increase. PVP cannot be well coated on the surface of the BT powder, resulting in a large local powder size and poor dispersion effect. Therefore, the present invention adopts two-step addition of PVP to prepare barium titanate powder with narrow particle size distribution and good dispersibility.
[0014] In step S2 of the present invention, the pH of the mixed solution is adjusted to make the pH>12, and the titanium source and the barium source are subjected to hydrothermal or solvothermal reaction under alkaline conditions. The surface of the generated barium titanate particles is easy to adsorb polar solvent ions and the high-index crystal plane is exposed, so that the barium titanate powder has a higher surface energy, resulting in the barium titanate powder being easy to agglomerate and aggregate growth during the preparation process. Once the powder particles agglomerate, the particle size becomes uneven and the particle size distribution becomes wide, affecting the quality of the powder. The present invention adds PVP and adsorbs it on the surface of the barium titanate powder, and an adsorption layer is formed on the outside of the powder. This adsorption layer will generate a strong repulsive force when the particles are close to each other, hindering the agglomeration and bonding between the barium titanate particles, so that the powder is evenly dispersed and non-agglomerated.
[0015] The solid obtained in step S3 of the present invention is cubic barium titanate powder, and polyvinyl pyrrolidone is adsorbed on the surface of the cubic barium titanate powder. The barium titanate powder in step S4 of the present invention is tetragonal barium titanate.
[0016] Preferably, the barium source is selected from at least one of BaCl2, Ba(OH)2, Ba(NO3)2, barium acetate and barium acetate.
[0017] Preferably, the titanium source is selected from at least one of titanium tetrachloride, n-butyl titanate, metatitanic acid, titanium dioxide, titanium hydroxide, titanium isopropoxide and titanium isopropoxide.
[0018] Preferably, the weight average molecular weight of the polyvinyl pyrrolidone is 10,000-40,000.
[0019] Preferably, the step S1 is: mixing the barium source solution and part of the polyvinyl pyrrolidone solution, and then mixing with the titanium source solution to obtain a mixed solution.
[0020] Preferably, the solvents in the barium source solution, the polyvinyl pyrrolidone solution and the titanium source solution are selected from at least one of water and ethanol. In the present invention, the solvent can be any organic solvent that can dissolve the barium source, the titanium source and the polyvinyl pyrrolidone. Based on environmental protection, cost and safety considerations, the present invention preferably uses water, ethanol, and a mixture of ethanol and water as the solvent.
[0021] Preferably, in step S1, the mass ratio of the barium element in the barium source to the part of the polyvinyl pyrrolidone is 100:(0.7-7). The present invention does not consider the amount of solvent when calculating the mass ratio of the barium element in the barium source to the part of the polyvinyl pyrrolidone, and only uses the two pure chemical substances of the barium source and the polyvinyl pyrrolidone as the calculation basis.
[0022] Preferably, the mass percentage of the partial polyvinyl pyrrolidone is 10-40% based on the total mass percentage of polyvinyl pyrrolidone being 100%. The present invention does not consider the amount of solvent when calculating the mass percentage of polyvinyl pyrrolidone in step S1 and step S3, and only uses the pure chemical substance of polyvinyl pyrrolidone as the calculation basis.
[0023] Preferably, the molar ratio of barium in the barium source to titanium in the titanium source is (1.1-2): 1. In the present invention, the amount of solvent is not considered when calculating the molar ratio of barium in the barium source to titanium in the titanium source, and only the two pure chemical substances of the barium source and the titanium source are used as the calculation basis.
[0024] Preferably, the temperature increasing step in step S3 is to increase the temperature to 50-120° C. at a heating rate of 1-10° C. / min.
[0025] Preferably, the mixing reaction time in step S3 is 30 to 300 minutes.
[0026] Preferably, the mixing reaction step in step S3 is: performing a stirring mixing reaction at a stirring rate of 50 to 500 r / min.
[0027] Preferably, the calcination temperature in step S4 is 750-850°C.
[0028] Preferably, the calcination time in step S4 is 5 to 100 minutes.
[0029] Preferably, the concentration of the polyvinyl pyrrolidone solution is 10-80 g / L.
[0030] Preferably, the step of mixing and reacting with the remaining polyvinyl pyrrolidone solution in step S3 is: adding the remaining polyvinyl pyrrolidone solution dropwise at a dropping rate of 10 to 300 mL / min, and then mixing and reacting.
[0031] Preferably, the dripping rate of the remaining polyvinyl pyrrolidone solution is 10-100 mL / min.
[0032] In the present invention, if the PVP dropping speed is slow, the PVP content in the solution is too low, and the coating effect on the BT powder becomes poor; if the PVP solution dropping speed is too fast, the viscosity of the solution system increases, and the dispersant cannot well coat the BT powder, resulting in a large local powder size and poor dispersion effect. Therefore, the PVP dropping speed must be within an appropriate range to facilitate obtaining barium titanate powder with good dispersibility.
[0033] Preferably, the step of collecting the solid in step S3 is: filtering the mixed reaction product to obtain a filter cake; and washing and drying the filter cake to obtain.
[0034] Preferably, the cleaning step is to disperse the filter cake in water, ultrasonicate it, and then filter press it.
[0035] Preferably, the ultrasonic time is 20 to 30 minutes.
[0036] Preferably, the cleaning step is repeated at least once.
[0037] Preferably, the drying time is 60 to 300 minutes.
[0038] Preferably, the drying temperature is 60-200°C.
[0039] Preferably, the drying step adopts infrared drying.
[0040] Preferably, the step S3 is: raising the temperature to 50-120° C. at a heating rate of 1-10° C. / min, then dropping the remaining polyvinyl pyrrolidone solution at a dropping rate of 10-300 mL / min, mixing and reacting, and collecting the solid.
[0041] Preferably, the step S2 comprises: using alkaline solution to adjust the pH of the mixed solution to make the pH>12.
[0042] Preferably, the concentration of the alkali solution is 1-4 mol / L.
[0043] Preferably, the alkali in the alkali solution is selected from at least one of NaOH, KOH, Ba(OH)2, (CH3)4NOH and ammonia water.
[0044] Preferably, steps S1, S2 and S3 are all performed under the protection of an inert gas. Mixing under the protection of an inert gas can prevent the barium source from reacting with carbon dioxide in the air to generate barium carbonate impurities.
[0045] Preferably, the inert gas is selected from at least one of nitrogen, argon, helium, neon, krypton and xenon; more preferably, the inert gas is selected from at least one of nitrogen and argon.
[0046] The second aspect of the present invention provides a multilayer ceramic capacitor, which is made from raw materials including barium titanate powder prepared by the preparation method described in the first aspect of the present invention.
[0047] The third aspect of the present invention provides a method for preparing the barium titanate powder described in the first aspect of the present invention and / or application of the barium titanate powder prepared by the preparation method described in the first aspect of the present invention in ceramic products.
[0048] Preferably, the ceramic product includes a thermistor, a multilayer ceramic capacitor, an inductor, a sensor or a sensitive element.
[0049] The beneficial effects of the present invention are as follows: the present invention solves the problems of easy agglomeration of powder, excessive growth of grains, and uneven grain distribution in the preparation process of barium titanate powder by adding PVP in two steps, and PVP can generate gas during the calcination process, which further hinders the agglomeration of barium titanate particles, thereby obtaining barium titanate powder with good dispersibility, narrow particle size distribution, and high proportion of tetragonal phase, which meets the raw material requirements of high-end MLCC products.
[0050] The present invention obtains barium titanate powder with uniform particle morphology, uniform particle size, good dispersibility, high tetragonal phase ratio and large specific surface area by controlling parameters such as PVP concentration, addition amount, addition method, heating rate and calcination temperature. The preparation method of the present invention is simple and easy to operate, has a wide range of application, and can be mass-produced industrially. DETAILED DESCRIPTION
[0051] The specific implementation of the present invention is further described in detail below in conjunction with examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0052] The "normal temperature" in the examples and comparative examples of the present invention refers to any temperature within the range of 20°C to 35°C.
[0053] Example 1
[0054] This example provides a method for preparing barium titanate powder, some of the process parameters of which are shown in Table 1. The specific preparation steps in this example are as follows:
[0055] S1: Under nitrogen atmosphere and room temperature, BaCl2, polyvinyl pyrrolidone (PVP) with a weight average molecular weight of 20,000 and water are mixed to form a barium source solution in a reactor, the concentration of PVP is 50 g / L, the mass ratio of Ba to PVP in BaCl2 is 100:4, that is, PVP / Ba is 4%, and then the molar ratio of Ba to Ti is 1.5:1, the barium-titanium ratio is controlled, and titanium tetrachloride solution is added to the obtained barium source solution to obtain a mixed solution; the amount of PVP added in step S1 accounts for 20wt% of the total PVP content;
[0056] S2: Under nitrogen protection, add 2 mol / L NaOH to the mixed solution obtained in step S1 while stirring until the pH reaches 14;
[0057] S3: Place the reactor in a water bath, raise the temperature to 80°C at a heating rate of 5°C / min, and then add 50g / L of PVP solution to the reactor at 100mL / min, with the amount of the solution accounting for 80wt% of the total PVP content. The entire reaction is carried out under nitrogen atmosphere and stirring at a stirring frequency of 200r / min and a reaction time of 150min to obtain a suspension;
[0058] S4: filtering, washing and drying the suspension obtained in step S3 to obtain cubic barium titanate-polyvinyl pyrrolidone powder;
[0059] The suspension needs to be filtered in a filter press device first, the filter cake is dissolved in pure water, stirred and ultrasonicated for 25 minutes, filtered again, and washed repeatedly. When the conductivity of the filtrate is less than 10μs / cm, the washing is completed and infrared drying is performed. The drying temperature is 100°C and the drying time is 100 minutes.
[0060] S5: calcining the cubic barium titanate-polyvinyl pyrrolidone powder obtained in step S4 at 800° C. for 30 min in air to obtain tetragonal barium titanate powder.
[0061] Embodiments 2 to 5
[0062] The only difference between the preparation methods of barium titanate powder in Examples 2 to 5 and that in Example 1 is that the concentration of PVP is different from that in Example 1.
[0063] Embodiments 6 to 9
[0064] The method for preparing barium titanate powder in Examples 6 to 9 is different from that in Example 1 only in that the ratio of PVP / Ba in step S1 is different from that in Example 1.
[0065] Embodiments 10 to 12
[0066] The preparation methods of barium titanate powder in Examples 10 to 12 are different from those in Example 1 only in that the mass percentage of PVP added for the first time in step S1 and the mass percentage of PVP added for the second time in step S3 are different from those in Example 1.
[0067] Examples 13 to 19
[0068] The only difference between the preparation methods of barium titanate powder in Examples 13 to 19 and that in Example 1 is that the dropping rate of PVP in step S3 is different from that in Example 1.
[0069] Comparative Examples 1-2
[0070] The preparation method of the barium titanate powder in Comparative Examples 1-2 is different from that in Example 1 only in that the concentration of PVP is different from that in Example 1.
[0071] Comparative Examples 3-4
[0072] The only difference between the preparation methods of barium titanate powder in Comparative Examples 3 to 4 and Example 1 is that the ratio of PVP / Ba in step S1 is different from that in Example 1.
[0073] Comparative Examples 5-6
[0074] The preparation method of barium titanate powder in Comparative Examples 5 to 6 is different from that in Example 1 only in that the mass percentage of PVP added for the first time in step S1 and the mass percentage of PVP added for the second time in step S3 are different from those in Example 1.
[0075] Comparative Examples 7 to 8
[0076] The only difference between the preparation method of barium titanate powder in Comparative Examples 7 to 8 and that in Example 1 is that the dropping rate of PVP in step S3 is different from that in Example 1.
[0077] Some process parameters in the preparation methods of barium titanate powders of Examples 1 to 19 and Comparative Examples 1 to 8 are shown in Table 1 below.
[0078] Table 1 Process parameters in the preparation methods of Examples 1 to 19 and Comparative Examples 1 to 8
[0079]
[0080]
[0081] Embodiments 20 to 23
[0082] The method for preparing barium titanate powder in Examples 20 to 23 is different from that in Example 1 only in that the heating rate in step S3 is different from that in Example 1.
[0083] Embodiments 24 to 26
[0084] The only difference between the preparation methods of barium titanate powder in Examples 24 to 26 and that in Example 1 is that the reaction temperature in step S3 is different from that in Example 1.
[0085] Examples 27 to 30
[0086] The only difference between the preparation methods of barium titanate powder in Examples 27 to 30 and that in Example 1 is that the reaction time in step S3 is different from that in Example 1.
[0087] Examples 31-32
[0088] The preparation method of barium titanate powder in Examples 31 to 32 is different from that in Example 1 only in that the calcination temperature in step S5 is different from that in Example 1.
[0089] Embodiments 33 to 35
[0090] The preparation method of barium titanate powder in Examples 33 to 35 is different from that in Example 1 only in that the calcination time in step S5 is different from that in Example 1.
[0091] Comparative Examples 9 to 10
[0092] The only difference between the preparation method of barium titanate powder in Comparative Examples 9 to 10 and that in Example 1 is that the heating rate in step S3 is different from that in Example 1.
[0093] Comparative Examples 11-12
[0094] The only difference between the preparation method of barium titanate powder in Comparative Examples 11 to 12 and that in Example 1 is that the reaction temperature in step S3 is different from that in Example 1.
[0095] Comparative Examples 13-14
[0096] The only difference between the preparation method of barium titanate powder in Comparative Examples 13 to 14 and that in Example 1 is that the reaction time in step S3 is different from that in Example 1.
[0097] Comparative Examples 15-16
[0098] The preparation method of the barium titanate powder in Comparative Examples 15 to 16 is different from that in Example 1 only in that the calcination temperature in step S5 is different from that in Example 1.
[0099] Comparative Examples 17-18
[0100] The preparation method of the barium titanate powder in Comparative Examples 17 to 18 is different from that in Example 1 only in that the calcination time in step S5 is different from that in Example 1.
[0101] Some process parameters in the preparation methods of barium titanate powders of Example 1, Examples 20 to 35 and Comparative Examples 9 to 18 are shown in Table 2 below.
[0102] Table 2 Process parameters in the preparation methods of Example 1, Examples 20 to 35 and Comparative Examples 9 to 18
[0103]
[0104]
[0105] Performance Test:
[0106] The particle size, particle size distribution and c / a value of the barium titanate powders prepared in Examples 1 to 35 and Comparative Examples 1 to 18 were tested respectively. The specific testing methods are as follows:
[0107] a)c / a
[0108] Standard: c / a>1.00950
[0109] Test method: XRD spectrum is measured by XRD instrument, and the tetragonal phase ratio c / a value is calculated through XRD diffraction pattern. The c / a value refers to the ratio of the a-axis length (a) and the c-axis length (c) of the barium titanate lattice constant, that is, the lattice constant ratio c / a. The closer the lattice constant ratio c / a is to 1, the closer the crystal form is to the cubic phase lattice, and the larger the lattice constant ratio c / a is, indicating that the crystal form is a tetragonal phase crystal form.
[0110] b) Particle size of barium titanate powder
[0111] Standard: 110-190nm
[0112] Test method: The average particle size of the particles is measured by observing the photos using a scanning electron microscope.
[0113] c) Dispersibility, i.e. the width of particle size distribution (D 90 -D 10 ) / D 50
[0114] Standard: Particle size distribution (D 90 -D 10 ) / D 50 <0.9
[0115] Test method: The particle size is measured by using a scanning electron microscope to observe the photo, and the probability distribution diagram is made by software. The data of particles at 10%, 50%, and 90% are taken to calculate the particle size distribution width.
[0116] d) Specific surface area of barium titanate powder
[0117] Standard: 7-8m 2 / g
[0118] Test method: The BET specific surface area of barium titanate powder was detected using a specific surface area and micropore physical adsorption instrument.
[0119] The performance data of the barium titanate powders of Examples 1 to 19 and Comparative Examples 1 to 8 measured according to the above test method are shown in Table 3 below.
[0120] Table 3 Performance data of barium titanate powders of Examples 1 to 19 and Comparative Examples 1 to 8
[0121] serial number c / a Particle size / μm Dispersibility <![CDATA[Specific surface area / m 2 / g]]> Example 1 1.00986 148 0.396 7.881 Example 2 1.00951 179 0.613 7.402 Example 3 1.00961 168 0.417 7.501 Example 4 1.00972 182 0.421 7.389 Example 5 1.00955 163 0.512 7.549 Example 6 1.00991 188 0.793 7.488 Example 7 1.00956 176 0.513 7.527 Example 8 1.00967 139 0.469 7.915 Example 9 1.00953 151 0.865 7.839 Example 10 1.00962 185 0.595 7.309 Embodiment 11 1.00963 141 0.436 7.833 Example 12 1.00975 156 0.477 7.656 Embodiment 13 1.01010 189 0.751 7.198 Embodiment 14 1.01002 181 0.633 7.183 Example 16 1.00958 134 0.496 7.977 Embodiment 17 1.00978 156 0.559 7.793 Embodiment 18 1.00982 179 0.618 7.465 Embodiment 19 1.00993 186 0.798 7.298 Comparative Example 1 1.00850 151 0.982 7.805 Comparative Example 2 1.00996 291 0.617 5.451 Comparative Example 3 1.00999 226 0.874 5.928 Comparative Example 4 1.00963 177 1.103 6.655 Comparative Example 5 1.01001 218 0.969 5.321 Comparative Example 6 1.00921 181 0.986 7.199 Comparative Example 7 1.00981 215 1.012 6.511 Comparative Example 8 1.00962 231 0.561 6.130
[0122] As can be seen from Table 3, by comparing Examples 1 to 5 and Comparative Examples 1 to 2, when the concentration of PVP is too low, the actual amount added during the secondary dropwise addition is small, the coating effect on the BT powder is poor, and the dispersibility is poor; when the PVP concentration is too high, the amount added in a short time during the secondary dropwise addition is too much, and the PVP self-crosslinking phenomenon occurs, resulting in the powder particle size being too large and the specific surface area being too small, which is difficult to meet the use requirements. By comparing Examples 6 to 9 and Comparative Examples 3 to 4, it can be seen that when the PVP / Ba ratio is too low, that is, when Ba is too much or PVP is too little, PVP forms undersaturated adsorption on the particle surface and cannot completely cover the entire surface of the barium titanate particles. Several particles are connected together through the cross-linking effect, causing particle agglomeration, a larger particle size, and a smaller specific surface area; when the PVP / Ba ratio is too high, that is, when Ba is too little or PVP is too much, extrusion occurs between molecules, and excess free molecular chains in the solution will be entangled with each other, causing the viscosity of the system to increase, further hindering the growth of small BT particles, so that the barium titanate powder particle size is small, the specific surface area is also small, and the dispersibility is very poor. By comparing Examples 10 to 12 with Comparative Examples 5 to 6, it can be seen that when the amount of PVP added in the first stage is too little, in the reaction temperature rising stage, the coating effect of PVP on the powder is poor, and grain agglomeration is prone to occur, the grain size is too large, the specific surface area is small, and the powder dispersibility is poor; when the amount of PVP added in the first stage is too much, the system viscosity is large, the particles are difficult to move, the nucleated particles are easy to aggregate, and the dispersibility is poor; by comparing Examples 13 to 19 with Comparative Examples 7 to 8, it can be seen that the dripping acceleration of PVP also affects the dispersion of grains, the particle size of grains, the specific surface area of grains and other parameters through the coating of BT and the change of system viscosity.
[0123] The performance data of the barium titanate powders of Example 1, Examples 20 to 35 and Comparative Examples 9 to 18 measured according to the above test method are shown in Table 4 below.
[0124] Table 4 Performance data of barium titanate powders of Example 1, Examples 20 to 35 and Comparative Examples 9 to 18
[0125]
[0126]
[0127] As shown in Table 4, by comparing Example 1, Examples 20-23, Examples 27-30 and Comparative Examples 9-10, Comparative Examples 13-14, it can be seen that the slow heating rate and the extended reaction time are conducive to grain growth, but the heating rate is too slow or the reaction time is too long, the grains grow too large, and the specific surface area does not meet the requirements. When the heating rate is too fast or the reaction time is too short, the powder is heated unevenly, some grains have grown, and some grains have just started to grow, so the overall dispersion of the powder is poor or there is a problem with the c / a value. By comparing Examples 24-26 and Comparative Examples 11-12, it can be seen that the higher the reaction temperature, the larger the grains, and the corresponding c / a. When the temperature is too high or too low, the grain size and c / a value will not meet the requirements. By comparing Examples 31 to 35 and Comparative Examples 15 to 18, it can be seen that increasing the calcination temperature or extending the calcination time is beneficial to the growth of grains and the increase of c / a, but calcining temperature that is too low or too high, or calcining time that is too long or too short, will result in grain size, specific surface area and c / a value that do not meet the requirements.
[0128] In summary, the preparation method of barium titanate powder in the present invention achieves the particle size range of 110 to 190 nm and the particle size distribution (D 90 -D 10 ) / D 50 <0.9, specific surface area is 7~8m 2 / g of tetragonal barium titanate powder, the barium titanate powder has small grains, uniform particle morphology, narrow particle size distribution, good dispersibility, high specific surface area, and a high proportion of tetragonal phase. The ceramic products made from the barium titanate powder have excellent performance and good mechanical properties.
[0129] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing barium titanate powder, Features: The following steps are involved: S1: mixing the barium source solution, part of the polyvinyl pyrrolidone solution, and the titanium source solution to obtain a mixed solution; S2: adjusting the pH of the mixed solution to make the pH>12; S3: heating, then mixing with the remaining polyvinyl pyrrolidone solution for reaction, and collecting the solid; S4: calcining the solid to obtain the barium titanate powder.
2. The method for preparing barium titanate powder according to claim 1, Features: The barium source is selected from BaCl 2 、Ba(OH) 2 ,Ba(NO 3 ) 2 , barium acetate, and at least one of barium acetate; And / or, the titanium source is at least one selected from titanium tetrachloride, n-butyl titanate, metatitanic acid, titanium dioxide, titanium hydroxide, titanium isopropoxide, and titanium isopropoxide; And / or, the weight average molecular weight of the polyvinyl pyrrolidone is 10,000 to 40,000.
3. The method for preparing barium titanate powder according to claim 1, Features: In the step S1, the mass ratio of the barium element in the barium source to the portion of the polyvinyl pyrrolidone is 100:(0.7-7); and / or, Taking the total mass percentage of polyvinyl pyrrolidone as 100%, the mass percentage of the partial polyvinyl pyrrolidone is 10-40%; and / or, The molar ratio of barium in the barium source to titanium in the titanium source is (1.1-2):
1.
4. The method for preparing barium titanate powder according to claim 1, Features: The heating step in step S3 is to raise the temperature to 50-120°C at a heating rate of 1-10°C / min; And / or, the mixing reaction time in step S3 is 30 to 300 minutes; And / or, the mixing reaction step in step S3 is: stirring and mixing the mixture at a stirring rate of 50 to 500 r / min; And / or, the calcination temperature in step S4 is 750-850° C., and the calcination time is 5-100 min.
5. The method for preparing barium titanate powder according to claim 1, Features: The concentration of the polyvinyl pyrrolidone solution is 10-80 g / L.
6. The method for preparing barium titanate powder according to claim 5, Features: The step of mixing and reacting with the remaining polyvinyl pyrrolidone solution in step S3 is: adding the remaining polyvinyl pyrrolidone solution dropwise at a dropping rate of 10 to 300 mL / min, and then mixing and reacting.
7. The method for preparing barium titanate powder according to claim 1, Features: The step S2 is: using alkaline solution to adjust the pH of the mixed solution to make the pH>12; the alkali in the alkaline solution is selected from NaOH, KOH, Ba(OH) 2 , (CH 3 ) 4 At least one of NOH and ammonia water.
8. The method for preparing barium titanate powder according to any one of claims 1 to 7, Features: The steps S1, S2 and S3 are all carried out under the protection of inert gas.
9. A multilayer ceramic capacitor, Features: The invention is prepared from raw materials including barium titanate powder prepared by the preparation method according to any one of claims 1 to 8.
10. The method for preparing the barium titanate powder according to any one of claims 1 to 8 and / or the use of the barium titanate powder obtained by the method according to any one of claims 1 to 8 in ceramic products.
Citation Information
Cited By
Preparation method of barium titanate powder
CN120682028A
Preparation method of barium titanate powder
CN121591249A
A method for preparing barium titanate powder
CN121591249B