Preparation method of biochar-loaded cellulose-grafted acrylic acid stabilized nano-iron

By polymerizing cellulose grafted acrylic acid in situ on biochar, the biochar-loaded cellulose grafted acrylic acid-stabilized nanoferric composite material was formed, which solved the problem of agglomeration and poor stability of nano zero-valent iron in water treatment, and achieved efficient removal The effect of hexavalent chromium.

CN118929834AInactive Publication Date: 2024-11-12YULIN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411279688.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The dispersion and stability of nano zero-valent iron in water treatment is poor due to agglomeration, which affects its removal efficiency of heavy metal chromium. The existing surface modification methods may lead to uneven coating thickness and hinder reaction mass transfer.

Method used

Using cellulose-grafted acrylic acid as a support, the in-situ polymerization on biochar by reverse phase suspension method and liquid phase reduction method to generate biochar-loaded cellulose-grafted acrylic acid-stabilized nanoferrous composite material, which improves the dispersion of nano zero-valent iron and stability.

Benefits of technology

Improve the reduction performance and stability of nano zero-valent iron, achieve efficient removal of hexavalent chromium, and reduce the agglomeration and oxidation of nano zero-valent iron through the loading and polymer coating of biochar, and improve the material Antioxidant properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929834A_ABST
    Figure CN118929834A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of functional materials and water treatment, in particular to a preparation method of biochar-loaded cellulose-grafted acrylic acid stabilized nano-iron, which comprises the following steps: firstly, pyrolyzing and modifying jujube branches to prepare biochar; then cellulose grafted acrylic acid prepared by a reversed-phase suspension method and biochar loaded nano zero-valent iron prepared by a liquid-phase reduction method are subjected to in-situ polymerization to generate nano zero-valent iron, the biochar is used as a carrier, the nano zero-valent iron is loaded, and the biochar used as the carrier can play a certain role in improving agglomeration of the nano iron; and the reduction performance of the nano zero-valent iron is improved to a certain extent. And the high polymer material cellulose grafted acrylic acid is used as the surface modifier of the nano zero-valent iron, so that the agglomeration and oxidation of the nano zero-valent iron are reduced, the stability of the nano zero-valent iron is improved, and the aim of efficiently removing Cr (VI) is fulfilled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional materials and water treatment, and more specifically, to a method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron. Background Art

[0002] The continuous development of industry has intensified the discharge of heavy metal ions, resulting in a large amount of wastewater containing these heavy metal ions being discharged into water bodies, posing a direct threat to people's drinking water hygiene. Therefore, people are paying more and more attention to the harm of heavy metal ions to human health and the environment. Heavy metal ions accumulate in organisms along the food chain, causing serious health problems for organisms. Although trace amounts of certain heavy metals play an important role in the human body's metabolism, they are toxic at high concentrations and may cause serious physiological or neurological damage. Chromium is one of the heavy metal ions, which is highly toxic. It mainly comes from industrial wastewater such as mining, metallurgy, electroplating, steel manufacturing, and dyes. It is reported that in terms of electroplating wastewater, there are about tens of thousands of electroplating plants in the country, which discharge up to 4 billion cubic meters of chromium-containing wastewater each year.

[0003] Chromium pollution is not limited to chromium ions. The number of pollutants in chromium-containing wastewater is large and the composition is complex. If the wastewater is discharged directly without treatment, these pollutants will directly enter the water environment, pollute groundwater sources and natural wastewater, and seriously affect human health and living environment safety. Chromium exists in various forms in the water environment, but as a redox metal element, most of it exists in the form of trivalent chromium (Cr(III)) and hexavalent chromium (Cr(VI)). Cr(VI) is highly toxic and mobile. It is considered to be a highly carcinogenic and teratogenic pollutant among environmental pollutants. Chromium in wastewater is usually present in the form of HCrO 4- , CrO4 2- and Cr2O7 2- Compared with Cr(VI), Cr(III) is less harmful and more stable, and generally exists in the form of oxides, hydroxides and inorganic salts. The two have different physical and chemical properties and toxicity, but they can be converted into each other through redox reactions. Therefore, it is of great significance to adopt effective remediation methods to reduce the concentration of heavy metal chromium to an acceptable limit.

[0004] In recent years, with the continuous development of materials science, nano zero-valent iron (nZVI) has been widely used in water treatment due to its large specific surface area, strong reducing ability, high efficiency, and low economic and environmental costs. It can effectively treat heavy metals in water bodies. In the field of water remediation, this high-functional nanomaterial water treatment method is an emerging method. When treating industrial wastewater containing heavy metal ions such as Cr(VI), Pb(II) and Cu(II), nZVI can be used to react these ions. Through redox reactions, they can be converted into harmless precipitates or adsorbed on the surface of the material to form co-precipitates. Due to its unique properties, nZVI is considered to be a new material with great application potential. At present, the research on nano zero-valent iron has attracted widespread attention.

[0005] Although nZVI itself has good reactivity, it tends to aggregate. To solve this problem, it is necessary to improve the process to improve dispersibility and reactivity, improve material properties and expand the scope of application. Therefore, nZVI modification research has been carried out based on the carrier method and surface modification method.

[0006] The loading method is to load nZVI evenly on other materials, which can effectively solve the problems of poor dispersion, durability, and mechanical properties caused by the aggregation of nano zero-valent iron, and achieve effective treatment of highly polluted water. This method utilizes the reduction and adsorption between nZVI and other carriers, while maintaining its reaction stability, it can also improve its antioxidant properties. [9] . Therefore, it is very important to select a green and environmentally friendly loading material with high protection ability for nZVI. The porous materials widely used in current research mainly include activated coke, zeolite, kaolin, activated carbon, biochar and graphene. Compared with other materials, biochar (BC) has the advantages of large specific surface area, stable structure and strong adsorption capacity. It is a readily available porous carbon-rich material. Biochar can be easily produced by pyrolysis of carbon-rich biomass under low oxygen conditions. In addition, the surface of biochar contains a large number of oxygen-containing groups, which are quite effective in adsorbing heavy metal ions.

[0007] The surface modification method is to modify the surface of nZVI using polymer composite materials to form a coating layer to protect nZVI, which can effectively increase the spatial barrier and electrostatic repulsion of nZVI, so that nZVI can be maintained in a smaller particle size range, thereby improving its dispersibility and stability in water and achieving efficient removal of Cr(VI). At present, this research field mainly uses polymer materials such as starch, chitosan, carboxymethyl cellulose (CMC), and polyvinyl pyrrolidone (PVP) to coat nZVI. We use cellulose grafted acrylic acid (Cell-g-PAA) to encapsulate nZVI. The main chain skeleton of Cell-g-PAA is cellulose, and its main chain and side chains contain functional groups such as hydroxyl and carboxyl groups, which can form complexes with heavy metal ion pollutants. Due to its good biodegradability, Cell-g-PAA is widely used in horticulture, environmental remediation and sanitation, and is considered to be a natural environment-friendly material.

[0008] Although loading and surface modification can improve the aggregation and catalytic activity of nano zero-valent iron, the loading rate of nano zero-valent iron is still low due to factors such as carrier structure and pore size, electrostatic repulsion, etc. Nano zero-valent iron is mainly distributed on the surface of the carrier, so it is easily destroyed by oxidation or other reasons. In addition, surface modification will also cause uneven thickness of the coating layer of the load. However, if the coating layer is too thick, it will hinder the mass transfer between nano zero-valent iron and Cr(VI), forming a physical barrier, thereby affecting the stability of nano zero-valent iron itself and its own reduction efficiency of heavy metal ions. Summary of the invention

[0009] To solve the above problems, the present invention provides a method for preparing biochar-loaded cellulose grafted acrylic acid-stabilized nano-iron, wherein cellulose grafted acrylic acid is used to coat biochar-loaded nano-zero-valent iron to obtain a biochar-loaded cellulose grafted acrylic acid-stabilized nano-iron composite material.

[0010] To achieve the above object, the technical solution adopted by the present invention is: A method for preparing biochar-loaded cellulose grafted acrylic acid-stabilized nano-iron, which firstly uses jujube branches to be pyrolyzed and modified to prepare biochar, and then uses cellulose grafted acrylic acid prepared by an inverse suspension method and biochar-loaded nano-zero-valent iron prepared by a liquid phase reduction method to be in-situ polymerized and generated, comprising the following steps: Step 1: Cut the jujube branches into small pieces, rinse them with deionized water several times to remove the surface dust, and then put them into the oven at 60 o C, dried for 6 h, crushed with a grinder, and passed through a 200-mesh sieve to obtain biomass powder; Step 2: Pour the prepared biomass powder into a 10 mL porcelain boat, then place it in a tube furnace, adjust the tube furnace heating rate to 20°C / min, and raise the reaction temperature to 500 o C. 600 o C. 700 o C, isothermal pyrolysis for 2 h to obtain biochar precursor; Step 3: Grind the biochar precursor and potassium hydroxide particles in a mortar at a mass ratio of 1:2, and then place them in a tube furnace. The tube furnace heating rate is adjusted to 20°C / min, and the reaction temperature is raised to 800 o C, biochar can be obtained by constant temperature pyrolysis for 2 h under N2 atmosphere; Step 4: Place 2.2 g of cellulose and 30 mL of distilled water in a four-necked flask equipped with an electric stirrer, a water bath, and a thermometer at 90 °C. o Gelatinize in water bath at 30 min. Step 5, slowly adding a certain amount of 5 mol / L NaOH solution into a beaker containing 14.4 mL acrylic acid solution using a rubber-tipped dropper for neutralization, and the neutralization reaction is carried out in an ice water bath; Step 6: Add dispersant and surfactant successively until the temperature drops to 40 o C. stirring the starch gelatinized liquid obtained in step 4, and introducing an inert gas to maintain an inert atmosphere throughout the reaction process; Step 7: add the initiator, suspension and crosslinking agent to the system prepared in step 6 in sequence, and heat to the polymerization temperature of 70°C under continuous stirring. o C was subjected to inverse suspension polymerization for 3 h; Step 8, after the reaction is completed, wash with ethanol and place in 60 o C oven for drying for 24 h, grinding after drying, and passing through a 200-mesh sieve to obtain a cellulose grafted polymer material; Step 9, placing the biochar prepared in step 3, ferrous sulfate heptahydrate, and sodium borohydride in a mass ratio of 1:5:3 in a four-necked flask filled with 150 mL of distilled water, stirring vigorously, and passing high-purity nitrogen before and after the reaction to remove dissolved oxygen in the water; Step 10, dissolving the cellulose graft polymerization monomer material obtained in step 8 in 100 mL of distilled water, pouring into the four-necked flask in step 9, and stirring vigorously; Step 11, after the reaction is completed, separation, purification, and vacuum drying are performed to obtain the composite material target product. In order to maintain the activity of the product for a long time, the composite material obtained by vacuum drying can be kept in a nitrogen environment for standby use.

[0011] Furthermore, in step 1, the amount of jujube branches used is 5 g-10 g; in step 2, the particle size of the biomass powder is 200 mesh, and the pyrolysis condition is calcination for 2 h under N2 atmosphere.

[0012] Furthermore, in step 3, potassium hydroxide particles are used as a surface pore expansion modifier, and the added amount is twice the mass of the monomer.

[0013] Furthermore, the amount of the initiator is 4.3-8.6 mL of a 5 g / L solution, the amount of the cross-linking agent is 1.25-2.5 mL of a 5 g / L solution, and the amount of the surfactant is 0.06-0.12 g; the oil phase is composed of a dispersant; the volume ratio of water to the dispersant is 1:5, the amount of ferrous sulfate heptahydrate is 5-10 g, and the amount of sodium borohydride is 3-6 g; wherein the amount of biochar is 1-2 g.

[0014] Furthermore, in step 2, the reaction temperature is raised to 600 o C, time is 2 h, protective gas is N2.

[0015] Furthermore, the initiator is one of potassium persulfate, sodium persulfate or ammonium persulfate, preferably potassium persulfate, and the amount of the initiator is 8.6 mL of a 5 g / L solution.

[0016] Further, the surfactant is one of sorbitol glycerol fatty acid, polyglycerol fatty acid ester or glycerol oleate, preferably polyglycerol fatty acid ester, and the amount of the surfactant is 0.12g; Furthermore, the cross-linking agent is N,N , -Methylene bisacrylamide, this type of crosslinking agent allows the super absorbent to form a crosslinked or slightly crosslinked three-dimensional network in the bulk phase to improve the gel strength of the super absorbent. The amount of crosslinking agent used is 2.5 mL of a 5 g / L solution; Further, the cellulose is one of wood cellulose, microcrystalline cellulose or nanocellulose, preferably wood cellulose, and the amount of cellulose is 2.2 g; Furthermore, the dispersant is n-hexane, and the stirring speed is 200-400 rpm.

[0017] The present invention has the following beneficial effects: 1. The present invention uses biomass - discarded jujube tree branches as raw materials, which are widely available and inexpensive, and can achieve effective utilization of waste.

[0018] 2. The present invention uses biomass jujube branches to prepare biochar by pyrolysis. Compared with other materials, biochar has the advantages of large specific surface area, stable structure, strong adsorption capacity, etc., and is a readily available porous carbon-rich material. There are abundant functional groups on the surface of biochar, including carboxyl, hydroxyl, ether, etc., which are quite effective in adsorbing heavy metal ions.

[0019] 3. The composite material prepared by the present invention uses biochar as a carrier to load nano-zero-valent iron. The biochar as a carrier can improve the aggregation of nano-iron to a certain extent, and improve the reduction performance of nano-zero-valent iron to a certain extent. In addition, the polymer material cellulose grafted with acrylic acid is used as a surface modifier of nano-zero-valent iron, which is beneficial to reduce the aggregation and oxidation of nano-zero-valent iron and improve the stability of nano-zero-valent iron, thereby achieving the goal of efficiently removing Cr(VI). BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings: Figure 1 The present invention is a flowchart of a method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to an embodiment of the present invention.

[0021] Figure 2 XRD pattern of the sample In the figure: (a) original biochar; (b) nano-zero-valent iron; (c) biochar loaded with nano-zero-valent iron; (d) biochar loaded with cellulose grafted with acrylic acid stabilized nano-zero-valent iron; (e) sample after adsorption.

[0022] Figure 3 is the FT-IR spectrum of the sample; In the figure: (a) original biochar; (b) modified biochar; (c) biochar loaded with nano zero-valent iron; (d) biochar loaded with cellulose grafted with acrylic acid stabilized nano zero-valent iron; (e) sample after adsorption.

[0023] Figure 4 is the SEM image of the sample; In the figure: (a) original biochar; (b) nano-zero-valent iron; (c) biochar loaded with nano-zero-valent iron; (d) cellulose grafted with acrylic acid; (e) biochar loaded with cellulose grafted with acrylic acid to stabilize nano-zero-valent iron; (f) sample after adsorption.

[0024] Figure 5 is the XPS graph of the sample; In the figure: (a) XPS total spectrum; (b) O 1s; (c) Fe 2p; (d) Cr 2p.

[0025] Figure 6The effect of different material dosages on Cr(VI) removal.

[0026] Figure 7 Reusability of biochar-loaded cellulose-grafted acrylic acid-stabilized nano-zero-valent iron. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0028] Example 1 A method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron comprises the following steps: Step 1: Take 5 g to 10 g of jujube branches, cut them into small pieces, rinse them with deionized water several times to remove the surface dust, put them into the oven, and heat them at 60 o C, dried for 6 h, crushed with a grinder, and passed through a 200-mesh sieve to obtain biomass powder; Step 2: Pour the prepared biomass powder into a 10 mL porcelain boat, then place it in a tube furnace, adjust the tube furnace heating rate to 20°C / min, and raise the reaction temperature to 600 o C, the time was 2 h, the protective gas was N2, and the biochar precursor was obtained; Step 3: Grind the biochar precursor and potassium hydroxide particles in a mortar at a mass ratio of 1:2, and then place them in a tube furnace. The tube furnace heating rate is adjusted to 20°C / min, and the reaction temperature is raised to 800 o C, biochar can be obtained by constant temperature pyrolysis for 2 h under N2 atmosphere; Step 4: Place 2.2 g of cellulose and 30 mL of distilled water in a four-necked flask equipped with an electric stirrer, a water bath, and a thermometer at 90 °C. o Gelatinize in water bath at 30 min. Step 5, preparing a partially neutralized sodium acrylate solution: slowly adding a certain amount of 5 mol / L NaOH solution into a beaker containing 14.4 mL of acrylic acid solution using a rubber-tipped dropper for neutralization, and the neutralization reaction is carried out in an ice water bath; Step 6: Add dispersant and surfactant successively until the temperature drops to 40 o C. stirring the starch gelatinized liquid obtained in step 4, and introducing an inert gas to maintain an inert atmosphere throughout the reaction process; Step 7: add the initiator, suspension and crosslinking agent to the system prepared in step 6 in sequence, and heat to the polymerization temperature of 70°C under continuous stirring. o C was subjected to inverse suspension polymerization for 3 h; Step 8, after the reaction is completed, wash with ethanol and place in 60 o C oven for 24 h, and after drying, grind and pass through a 200-mesh sieve to obtain a cellulose-grafted sodium acrylate material; Step 9, placing the biochar prepared in step 3, ferrous sulfate heptahydrate, and sodium borohydride in a mass ratio of 1:5:3 in a four-necked flask filled with 150 ml of distilled water, stirring vigorously, and passing high-purity nitrogen before and after the reaction to remove dissolved oxygen in the water; Step 10, dissolving the cellulose grafted sodium acrylate material prepared in step 8 in 100 mL of distilled water, pouring into the four-necked flask in step 9, and stirring vigorously; Step 11, after the reaction is completed, separation, purification and vacuum drying are performed to obtain the target composite material product.

[0029] In this embodiment, in step 3, potassium hydroxide particles are used as a surface pore expansion modifier, and the amount added is twice the mass of the monomer. The initiator is potassium persulfate, and the amount of the initiator is 8.6 mL of a 5 g / L solution; the surfactant is polyglycerol fatty acid ester, and the amount of the surfactant is 0.12 g; the crosslinking agent is N,N , -methylenebisacrylamide, the amount of the cross-linking agent is 2.5 mL of a 5 g / L solution; the cellulose is wood cellulose, the amount of which is 2.2 g; the dispersant is n-hexane, the volume ratio of water to the dispersant is 1:5, the stirring speed is 300 rpm, the amount of ferrous sulfate heptahydrate is 5 g, the amount of sodium borohydride is 3 g, and the amount of biochar is 1 g.

[0030] The present invention utilizes the surface modification and loading method to improve the stability and activity of nano zero-valent iron, which can be confirmed from the XRD, FT-IR, SEM and XPS spectra of biochar, nano zero-valent iron, and biochar loaded cellulose grafted acrylic acid stabilized nano iron.

[0031] XRD( Figure 2 ) are the XRD spectra of BC-nZVI@Cell-g-PAA, BC-nZVI@Cell-g-PAA, BC-nZVI, nZVI and BC powder after adsorption. It can be seen from the figure that the XRD spectrum of BC at 2θ=26 o and 2θ = 43.1 oThere are two peaks near the graphite structure of carbon (002) and (100) planes. The XRD spectra of nZVI, BC-nZVI and BC-nZVI@Cell-g-PAA show that Fe 0 The characteristic peak (2θ=44.67 o ), compared with the PDF standard card, it shows that the prepared nano-iron is nano-element zero-valent iron. Compared with nZVI, BC-nZVI has a lower content of Fe in BC-nZVI due to the loading of biochar. 0 The diffraction intensity of BC-nZVI@Cell-g-PAA is greatly reduced. However, under the loading of BC and the coating of polymer materials, the Fe 0 The diffraction intensity decreased again. The XRD spectrum of BC-nZVI@Cell-g-PAA after adsorption showed an obvious diffraction peak at 2θ=14.16 o , 2θ=27.07 o , 2θ=36.24 o , 2θ=46.76 o , pointing to the (020), (120), (031) and (051) crystal planes respectively. These peaks are FeO(OH) peaks after comparison with the PDF standard card, indicating that the appearance of FeO(OH) after the reaction is a redox reaction.

[0032] FT-IR images ( Figure 3 ) are the FT-IR spectra of BC-nZVI@Cell-g-PAA, BC-nZVI@Cell-g-PAA, BC-nZVI, BC after pore expansion and original BC after adsorption. By comparing the infrared spectra, the functional groups on the surfaces of different samples can be qualitatively analyzed. At 3430 cm -1 The characteristic absorption peak at 1620 cm is the stretching vibration band of -OH. -1 The peak at 1720 cm represents the C=C bond. -1 The characteristic peaks near 1160 cm -1 The bands nearby are associated with CO bending vibrations. About 867 cm -1 The weak band at is due to the bending vibration of CH. The peak intensity of oxygen-containing functional groups such as -OH, C=O and CO of the synthesized sample BC-nZVI@Cell-g-PAA is significantly stronger than that of BC. From the above analysis, it can be seen that BC-nZVI@Cell-g-PAA prepared by in situ polymerization-liquid phase reduction has more oxygen-containing functional groups, which can promote the adsorption of Cr(VI) ions in the solution, thereby showing the characteristics of rapid removal.

[0033] From the SEM analysis of the samples ( Figure 4 ), it can be seen from the figure that the original BC powder ( Figure 4 a) The surface is rough and porous, and its large number of pores provide favorable conditions for the subsequent preparation of composite materials. nZVI can be better loaded on the surface or pores of BC. nZVI ( Figure 4 b) Because the spherical particles of nZVI are distributed in the form of chains, they show typical agglomeration phenomenon, which is due to the high surface energy and inherent magnetic interaction between the particles. BC-nZVI ( Figure 4 c) In the composite material, nZVI is evenly dispersed on the surface of BC, providing more adsorption reaction sites for hexavalent chromium. There is not much agglomeration of nZVI on the surface of BC, and some of them are larger particles. Some nZVI is attached to the pores of BC, which makes nZVI effectively fixed during the reaction and avoids the loss of nZVI in the reaction. From the SEM image of BC-nZVI@Cell-g-PAA ( Figure 4 e) It can be seen that many flocs are produced on the surface of biochar, indicating that the biochar and cellulose-grafted acrylic acid interact with each other through the encapsulation method, and nZVI is also evenly dispersed on the surface of biochar, which further indicates that BC-nZVI@Cell-g-PAA prepared by the method of first loading and then encapsulation can effectively play the role of nano zero-valent iron in removing Cr(VI), and at the same time, the surface nZVI is encapsulated by Cell-g-PAA, and the anti-oxidation performance of the material is also improved; by comparison (Appendix Figure 4 e and 4f) SEM images of the composite material before and after removal of Cr(VI) show that the floccules on the surface of BC-nZVI@Cell-g-PAA increased after the reaction. This is because during the entire adsorption process, Fe 0 The surface of the Cr(VI) is covered by Fe(OH)2, Fe(OH)3 and Cr(OH)3 precipitation layers generated by continuous oxidation and reduction of Cr(VI).

[0034] Figure 5 XPS analysis was performed on BC-nZVI@Cell-g-PAA before and after the reaction with Cr(VI) to obtain the surface information of the composite material before and after the reaction with Cr(VI). Figure 5 a The typical characteristic peaks of O 1s, Fe 2p and Cr 2p were observed respectively, which clearly confirmed that BC-nZVI@Cell-g-PAA was mainly composed of C, O and Fe. After reacting with Cr(VI), Cr 2p also appeared on the surface of the material, which was consistent with the SEM-EDS results. Then, narrow scans of O 1s, Fe 2p and Cr 2p were further performed to study the composition ratio and state of these elements. Figure 5From the XPS spectrum of b, it can be seen that O 1s has three peaks, with the peak centers located at 530.1 eV, 531.7 eV, and 533.2 eV, corresponding to the characteristic peaks of oxide (Fe-O), carbonyl and surface hydroxyl (CO / OH), and adsorbed water (H2O), respectively. FeO(OH) was generated after reaction with Cr(VI). From the figure, it can be seen that the peak intensity of phenolic OH and CO weakened after the reaction of BC-nZVI@Cell-g-PAA with Cr(VI), especially phenolic OH. As reported by Chen et al., after the complexation of phenolic OH and Cr(VI), the Mulliken charge of the aromatic ring increased significantly, enabling it to adsorb Cr(VI) through electrostatic interaction. From Figure 5 c From the Fe 2p spectrum before and after the reaction of BC-nZVI@Cell-g-PAA with Cr(VI), it can be seen that the peaks at the binding energies of 711.2 eV and 724.3 eV correspond to Fe 2p3 / 2 and Fe 2p1 / 2, respectively. In addition, it can be seen from the figure that the characteristic peaks at the binding energies of 711.2 eV and 724.3 eV correspond to Fe(II); the peaks at 713.7 eV and 726.8 eV correspond to Fe(III); the weak characteristic peaks at 707.3 eV and 720.3 eV correspond to Fe 0 ; The peaks at 718.8eV and 729.5eV correspond to satellite peaks. Figure 5 c shows that the Fe on the outer surface of BC-nZVI@Cell-g-PAA material before the reaction 0 and Fe(II) accounted for 5.1% and 78.2%, respectively, and Fe(III) accounted for 16.7%. After reacting with Cr(VI), Fe 0 The proportion of Fe(II) decreased to 64.1%, while the intensity of Fe(III) continued to increase, and the proportion increased to 35.9%, which indicates that Fe 0 and Fe(II) to reduce Cr(VI). Figure 5 d The Cr 2p spectrum after the reaction of BC-nZVI@Cell-g-PAA with Cr(VI) shows that the two peaks at 577.3 eV and 586.7 eV correspond to Cr(III) 2p 1 / 2 and Cr(III)2p 3 / 2 ; The two peaks at 580 eV and 589.3 eV correspond to Cr(VI)2p 3 / 2 and Cr(VI)2p 1 / 2. Among them, the proportion of Cr(III) accounts for 85.1%, and the proportion of Cr(VI) accounts for 14.9%. Cr(III) and Cr(III) exist simultaneously on the surface of the material after the reaction, which shows that the removal methods of Cr(VI) include physical adsorption and chemical reduction. The physical adsorption method adsorbs Cr(VI) to the surface of the material, and the chemical reduction method reduces Cr(VI) to Cr(III). The proportion of Cr(III) is much greater than that of Cr(VI), so the chemical reduction method is mainly used in the process of removing Cr(VI).

[0035] Research methods for treating hexavalent chromium polluted water Spectrophotometry uses diphenylcarbohydrazide as a colorimetric agent. Under acidic conditions, hexavalent chromium reacts with diphenylcarbohydrazide to produce a purple-red compound that can be directly detected by spectrophotometry.

[0036] Specific research methods: (1) Weigh 1 g of sample and add it into a 250 ml conical flask. Pour 100 ml (50 mg / L) of chromium experimental solution into the conical flask and seal it with plastic wrap.

[0037] (2) Place in a dual-function constant temperature water bath oscillator at a temperature of 25 o C. Oscillate at a speed of 150 r / min for two hours.

[0038] (3) When the reaction reaches adsorption equilibrium, use a syringe to weigh 10 ml of water sample, filter it through a microporous filter membrane, and transfer 1 ml of the filtrate into a 50 ml colorimetric tube and dilute to the scale line.

[0039] (4) Then add 1+1 sulfuric acid and phosphoric acid, then add 2 ml of the color developer solution and shake well.

[0040] (5) After standing for 5 to 10 minutes, use a 3 cm colorimetric dish and water as a reference to measure the absorbance at a wavelength of 540 nm using an ultraviolet spectrophotometer. The concentration of hexavalent chromium is thus determined, and the removal rate is calculated using formula (1).

[0041] (1) Where R is the removal rate (%), C0 is the initial concentration of hexavalent chromium (mg / L), and C t is the hexavalent chromium concentration at time t.

[0042] By attaching Figure 6 It can be seen that the different addition amounts of six materials, namely, biochar, modified biochar, biochar-loaded nano-zero-valent iron, biochar-loaded cellulose grafted acrylic acid-stabilized nano-zero-valent iron (carbon-iron ratio = 1:0.5), and biochar-loaded cellulose grafted acrylic acid-stabilized nano-zero-valent iron (carbon-iron ratio = 1:1), showed significant differences in adsorption performance at the adsorption temperature of 25o C. The removal effect of 50 mg / L Cr(VI) wastewater solution under the conditions of adsorption time of 2 h and rotation speed of 150 r / min. When the dosage of different materials is increased, the removal rate of Cr(VI) is continuously improved. Figure 6 It can be seen that the removal efficiency of biochar loaded with cellulose grafted with acrylic acid stabilized nano-zero-valent iron (carbon-iron ratio = 1:1) is the highest, and the removal rate tends to be flat as the dosage increases. In addition, the reuse performance was evaluated. Figure 7 As we know, the removal rate of materials decreases with repeated use. When used for the first time, 2.5 g / L BC-nZVI@Cell-g-PAA can achieve 100% chromium removal. After repeated use twice, although the removal effect is reduced, the removal rate can reach 82%.

[0043] From the above, it can be seen that BC-nZVI@Cell-g-PAA was prepared by in situ polymerization-liquid phase reduction method, which has a strong removal rate and the highest removal rate can reach 100%.

[0044] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron, characterized in that: The steps include: Step 1: Cut the jujube branches into small pieces, rinse them with deionized water several times to remove the surface dust, and then put them into the oven at 60 o C, dried for 6 h, crushed with a grinder, and passed through a 200-mesh sieve to obtain biomass powder; Step 2: Pour the prepared biomass powder into a 10 mL porcelain boat, then place it in a tube furnace, adjust the tube furnace heating rate to 20°C / min, and raise the reaction temperature to 500 o C. 600 o C. 700 o C, isothermal pyrolysis for 2 h to obtain biochar precursor; Step 3: Grind the biochar precursor and potassium hydroxide particles in a mortar at a mass ratio of 1:2, and then place them in a tube furnace. The heating rate of the tube furnace is adjusted to 20°C / min, and the reaction temperature is raised to 800 o C, biochar can be obtained by constant temperature pyrolysis for 2 h under N2 atmosphere; Step 4: Place 2.2 g of cellulose and 30 mL of distilled water in a four-necked flask equipped with an electric stirrer, a water bath, and a thermometer at 90 °C. o Gelatinize in a water bath at C for 30 min; Step 5, slowly adding a certain amount of 5 mol / L NaOH solution into a beaker containing 14.4 mL acrylic acid solution using a rubber-tipped dropper for neutralization, and the neutralization reaction is carried out in an ice water bath; Step 6: Add dispersant and surfactant successively until the temperature drops to 40 o C. stirring the starch gelatinized liquid obtained in step 4, and introducing an inert gas to maintain an inert atmosphere throughout the reaction process; Step 7: add the initiator, suspension and crosslinking agent to the system prepared in step 6 in sequence, and heat to the polymerization temperature of 70°C under continuous stirring. o C was subjected to inverse suspension polymerization for 3 h; Step 8, after the reaction is completed, wash with ethanol and place in 60 o C oven for drying for 24 h, grinding after drying, and passing through a 200-mesh sieve to obtain a cellulose grafted polymer material; Step 9, placing the biochar prepared in step 3, ferrous sulfate heptahydrate, and sodium borohydride in a mass ratio of 1:5:3 in a four-necked flask filled with 150 ml of distilled water, stirring vigorously, and passing high-purity nitrogen before and after the reaction to remove dissolved oxygen in the water; Step 10, dissolving the cellulose graft polymer material obtained in step 8 in 100 mL of distilled water, pouring into the four-necked flask in step 9, and stirring vigorously; Step 11, after the reaction is completed, separation, purification and vacuum drying are performed to obtain the target composite material product.

2. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: In the step 1, the amount of jujube branches used is 5 g-10 g; in the step 2, the particle size of the biomass powder is 200 mesh, and the pyrolysis condition is calcination for 2 h under N2 atmosphere.

3. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: In the step 3, potassium hydroxide particles are used as a surface pore expansion modifier, and the added amount is twice the weight of the monomer.

4. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The amount of the initiator is 4.3-8.6 mL of a 5 g / L solution, the amount of the cross-linking agent is 1.25-2.5 mL of a 5 g / L solution, and the amount of the surfactant is 0.06-0.12 g; the oil phase is composed of a dispersant; the volume ratio of water to the dispersant is 1:5, the amount of ferrous sulfate heptahydrate is 5-10 g, the amount of sodium borohydride is 3-6 g; and the amount of biochar is 1-2 g.

5. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: In step 2, the reaction temperature is raised to 600 o C, time is 2 h, protective gas is N2.

6. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The initiator is one of potassium persulfate, sodium persulfate or ammonium persulfate, and the amount of the initiator used is 8.6 mL of a 5 g / L solution.

7. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The surfactant is one of sorbitol glycerol fatty acid, polyglycerol fatty acid ester or glycerol uronic acid glycerol oleate, and the amount of the surfactant used is 0.12g.

8. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The cross-linking agent is N,N , -methylenebisacrylamide, 2.5 mL of a 5 g / L solution of crosslinker.

9. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The cellulose is one of wood cellulose, microcrystalline cellulose or nanocellulose, and the amount of cellulose used is 2.2 g.

10. The method for preparing biochar-loaded cellulose-grafted acrylic acid-stabilized nano-iron according to claim 1, characterized in that: The dispersant is n-hexane, and the stirring speed is 200-400 rpm.

Citation Information

Cited By

  • Soil structure modifier and preparation method thereof

    CN121674075A

  • A soil structure improver and a method of preparing the same

    CN121674075B