Preparation method of bending-resistant jumper cable material for rail car

By combining modified fillers with flame retardants, a stable hybrid network structure is formed, which solves the problem of poor compatibility of traditional flame retardants and achieves high-performance flame retardant and aging-resistant properties of cable materials for rail vehicles.

CN118931026APending Publication Date: 2024-11-12迈特诺技术股份有限公司
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411127238.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional magnesium hydroxide and aluminum hydroxide flame retardants have poor compatibility with the matrix resin in rail vehicle cable materials, resulting in a decline in mechanical and processing properties. Furthermore, the flame retardant properties of existing cable materials are not durable in fires.

Method used

Modified fillers (magnesium hydroxide, nano-silica, nano-titanium dioxide) were prepared by reacting with maleic anhydride and then combined with flame retardants containing phosphorus, silicon, and nitrogen elements to form a stable hybrid network structure through chemical action, thereby improving compatibility and flame retardant performance.

Benefits of technology

It improves the mechanical and flame-retardant properties of cable materials, providing long-lasting flame retardancy, anti-aging properties, and high mechanical strength, making it suitable for bending-resistant jumper cables for rail vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996791840000041
    Figure BDA0004996791840000041
  • Figure BDA0004996791840000042
    Figure BDA0004996791840000042
  • Figure BDA0004996791840000051
    Figure BDA0004996791840000051
Patent Text Reader

Abstract

The invention discloses a preparation method of a bending-resistant jumper cable material for a rail car, and belongs to the technical field of cable materials. The preparation method comprises the following steps: weighing 70-80 parts by weight of ethylene-vinyl acetate copolymer, 30-40 parts by weight of modified filler, 20-30 parts by weight of high density polyethylene, 10-20 parts by weight of elastomer, 10-15 parts by weight of flame retardant, 5-10 parts by weight of acrylate, 0.5-1 part by weight of antioxidant, 0.5-1 part by weight of ultraviolet light absorber, 0.5-1 part by weight of lubricant and 0.5-1 part by weight of initiator, uniformly mixing, putting into a double-screw extruder, mixing and granulating to obtain the cable material. The modified filler, the flame retardant, the ethylene-vinyl acetate copolymer, the acrylic ester and the polyethylene have chemical action and form a stable and firm hybrid network structure, so that the modified filler and the flame retardant can be fully dispersed in the cable material and play a role for a long time; therefore, the cable material disclosed by the invention has lasting and excellent flame-retardant effect, ageing-resistant characteristic and mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cable materials, and in particular relates to a method for preparing a bending-resistant jumper cable material for a rail vehicle. Background Art

[0002] As a supporting industry of the power industry, which is one of the pillar industries of the national economy, the wire and cable industry plays an extremely important role and position in the national economy. Bend-resistant jumper cables for rail vehicles need to have high bending resistance. Ethylene-vinyl acetate copolymer cable materials have the characteristics of good elasticity, light weight, strength, low shrinkage, etc. At the same time, they also have the advantages of good softness and excellent low temperature resistance. These characteristics make ethylene-vinyl acetate copolymer cable materials perform well in applications. Polyethylene cable materials are widely used in the field of wires and cables because of their light weight, good mechanical properties, very good low temperature resistance, good environmental stress cracking resistance, good processability, excellent electrical insulation performance, etc.

[0003] In addition, rail cars are usually crowded with people and the surrounding buildings are complex. Once a fire occurs, it is difficult to evacuate people and carry out rescue work. Therefore, the bending-resistant jumper cable material for rail cars needs to be added with a suitable flame retardant to give the cable material efficient, safe and long-lasting flame retardant properties. Although traditional magnesium hydroxide and aluminum hydroxide flame retardants can give the material good flame retardant properties, they have poor compatibility with the matrix resin and often reduce the mechanical properties and processing properties of the material. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a bending-resistant jumper cable material for a rail vehicle.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a bending-resistant jumper cable material for a rail vehicle comprises the following steps:

[0007] Weigh 70-80 parts of ethylene-vinyl acetate copolymer, 30-40 parts of modified filler, 20-30 parts of high-density polyethylene, 10-20 parts of elastomer, 10-15 parts of flame retardant, 5-10 parts of acrylate, 0.5-1 part of antioxidant, 0.5-1 part of ultraviolet absorber, 0.5-1 part of lubricant and 0.5-1 part of initiator by weight, put all the raw materials into a high-speed mixer and mix them evenly, then put them into a twin-screw extruder for mixing and granulation to obtain a cable material.

[0008] Furthermore, the modified filler is prepared by the following steps:

[0009] Under nitrogen protection, inorganic filler, DMAP (4-dimethylaminopyridine) and DMSO (dimethyl sulfoxide) were added to a three-necked flask, and the mixture was stirred until uniformly mixed. Maleic anhydride was then slowly added. After the addition was completed, the temperature was raised to 50°C, and the reaction was kept warm for 12 hours. After the reaction was completed, the mixture was centrifuged, and the centrifugal precipitate was first washed 3 times with deionized water and then washed 3 times with anhydrous ethanol to obtain a modified filler. The dosage ratio of inorganic filler, maleic anhydride, DMAP and DMSO was 10g:14-18g:3.5-4.5g:180mL.

[0010] Furthermore, the inorganic filler is a mixture of magnesium hydroxide, nano silicon dioxide and nano titanium dioxide in a mass ratio of 5:3:2.

[0011] When magnesium hydroxide is decomposed by heat, it releases bound water, which can not only absorb a large amount of latent heat to reduce the surface temperature of the material in the flame, but also inhibit the decomposition of polymers and cool combustible gases. In addition, the residual magnesium oxide produced by the decomposition of magnesium hydroxide is a dense oxide, which can be deposited on the surface of the material, inhibit the generation of combustible gases, play a role in heat insulation and oxygen isolation, and achieve the effect of smoke suppression. Magnesium hydroxide can also promote carbonization of the material surface, isolate oxygen from contact with the material, and further reduce the generation of smoke.

[0012] Nano silicon dioxide can significantly improve the mechanical strength of cable materials, enhance their wear resistance and tear resistance, thereby improving the service life and safety of cables. Nano titanium dioxide can not only absorb ultraviolet rays, but also reflect and scatter ultraviolet rays, and it has good chemical stability and light stability, and will not decompose or lose effectiveness due to light or chemical reactions. Therefore, the addition of nano titanium dioxide can significantly improve the weather resistance and aging resistance of cable materials and extend the service life of cables. In addition, nano titanium dioxide can also enhance the mechanical strength of cables, ensuring that the cables maintain stable performance during long-term use. Nano silicon dioxide and nano titanium dioxide work synergistically, and can jointly improve the mechanical properties of cable materials, thereby enabling the cable material of the present invention to be used as a bending-resistant jumper cable material for rail vehicles.

[0013] The surfaces of the three inorganic fillers, magnesium hydroxide, nano-silicon dioxide and nano-titanium dioxide, are rich in hydroxyl groups. Under the catalytic action of DMAP, the inorganic fillers can undergo esterification reaction with maleic anhydride to prepare modified fillers, so that the surface of the modified fillers is grafted with abundant carbon-carbon double bonds. Under the action of initiators, they can react chemically with the carbon-carbon double bonds of flame retardants and acrylates, and the unreacted carbon-carbon double bonds at the ends of polyethylene and ethylene-vinyl acetate copolymers, thereby greatly reducing the surface energy of the modified fillers and greatly improving the compatibility with other raw materials. The modified fillers can give full play to their own role and give the cable materials excellent mechanical properties, flame retardant and smoke suppression properties, and anti-ultraviolet effects.

[0014] Furthermore, the elastomer is one or more of ethylene-octene copolymer, ethylene-propylene copolymer, and ethylene-hexene copolymer.

[0015] Furthermore, the flame retardant is prepared by the following steps:

[0016] S1. Under nitrogen protection, flame retardant FRC-2 (3-[(hydroxymethyl)amino]-3-oxopropylphosphonic acid-dimethyl ester), pyridine and tetrahydrofuran dried over anhydrous calcium chloride were placed in a dry three-necked flask, stirred evenly, and then phosphorus oxychloride was slowly added. After the addition was completed, it was placed at 0°C for reaction for 0.5h. After the reaction was completed, centrifuged, the precipitate was dried, purified by column chromatography (the eluent was a mixed solvent of benzene and ether, and the volume ratio of benzene and ether was 4:6), and distilled under reduced pressure to obtain intermediate 1; the amount ratio of phosphorus oxychloride, flame retardant FRC-2, pyridine and tetrahydrofuran was 0.045mol:0.093mol:7.5mL:120mL;

[0017] Under the condition of pyridine as an acid binding agent, phosphorus oxychloride and flame retardant FRC-2 undergo esterification reaction, and the reaction process is as follows:

[0018]

[0019] S2. Under nitrogen protection, 2-methylene-1,3-propanediol, triethylamine and DMSO (dimethyl sulfoxide) were placed in a dry brown three-necked flask, stirred evenly, and then the mixed solution of intermediate 1 and DMSO was slowly added. After the addition was completed, the mixture was placed at 0°C for reaction for 1 hour. After the reaction was completed, the precipitate was centrifuged and dried. The precipitate was purified by column chromatography (the eluent was a mixed solvent of benzene and ethyl acetate, and the volume ratio of benzene and ethyl acetate was 1:1), and distilled under reduced pressure to obtain intermediate 2; the dosage ratio of intermediate 1, 2-methylene-1,3-propanediol, triethylamine and DMSO was 0.04 mol: 0.043 mol: 8.3 mL: 120 mL;

[0020] Under the condition of triethylamine as an acid-binding agent, intermediate 1 and 2-methylene-1,3-propanediol undergo esterification reaction, and the reaction process is as follows:

[0021]

[0022] S3, nitrogen was blown into a dry three-necked flask for 30 minutes to drive away the air in the flask, then intermediate 2 and DMF (N, N-dimethylformamide) were added, and after stirring and dissolving, octadecyltrichlorosilane was slowly added, and the system temperature was kept below 20°C. After the addition was completed, the temperature was raised to 30°C, and the reaction was kept warm for 6 hours. After the reaction was completed, it was cooled to room temperature, centrifuged, dried, purified by column chromatography (the eluent was a mixed solvent of chloroform and acetone, and the volume ratio of chloroform and acetone was 7:3), and the flame retardant was obtained by vacuum distillation. The amount ratio of intermediate 2, octadecyltrichlorosilane and DMF was 0.046mol:0.015mol:180mL.

[0023] Under heating conditions, intermediate 2 and octadecyltrichlorosilane undergo esterification reaction, and the reaction process is as follows:

[0024]

[0025] The flame retardant of the present invention contains abundant phosphate groups and halogen-free flame retardant elements nitrogen and silicon. The phosphate groups will undergo hydrolysis reaction at high temperature to generate phosphoric acid and methanol. The phosphoric acid can react with the free radicals generated by combustion to form a phosphorus oxide layer to prevent the contact between oxygen and fuel, thereby playing a flame retardant role; in addition, the phosphate compounds can decompose and absorb heat at high temperature, slow down the burning speed of the material, prolong the burning time, and improve the flame retardant performance of the material. This thermal stabilization effect helps to slow down the propagation speed of the flame and increase the flame retardant effect of the material. The flame retardant containing nitrogen elements releases non-combustible gases such as ammonia, nitrogen, deep nitrogen oxides, and water vapor after thermal decomposition. The generation of these gases and the decomposition of the flame retardant absorb heat and take away most of the heat, greatly reducing the surface temperature of the polymer; in addition, these non-combustible gases can also dilute the oxygen in the air and the concentration of combustible gases generated by the thermal decomposition of the polymer, and react with the oxygen in the air to generate nitrogen, water and deep oxides, consuming the oxygen on the surface of the material, thereby achieving a good flame retardant effect. During the combustion process, silicon-containing flame retardants can form a polymer gradient material with a surface enriched layer of organic silicon flame retardants. Once burned, it will generate an inorganic oxygen-isolating and heat-insulating protective layer containing Si bonds or Si-C bonds, which is unique to polysiloxane. This not only prevents the escape of combustion decomposition products, but also inhibits the thermal decomposition of polymer materials, achieving the purpose of flame retardancy, low smoke and low toxicity. In addition, silicon-containing flame retardants will generate non-flammable gases such as H2O and CO2 during combustion, diluting the oxygen concentration to achieve a synergistic flame retardant effect. Nitrogen, phosphorus and silicon elements work together through chemical reactions, physical isolation and gas phase coagulation to effectively improve the flame retardant properties of flame retardants.

[0026] The flame retardant contains a long carbon chain, which can be inserted into the ethylene-vinyl acetate copolymer and polyethylene macromolecular chain, thereby increasing the mechanical properties of the cable material. The flame retardant contains multiple carbon-carbon double bonds, which can react chemically with the double bonds on the surface of the modified filler under the action of the initiator, dispersing the modified filler while also dispersing itself. At the same time, the carbon-carbon double bonds on the surface of the flame retardant can also react chemically with the carbon-carbon double bonds of acrylates, and the carbon-carbon double bonds at the ends of polyethylene and ethylene-vinyl acetate copolymers that have not reacted completely, and then the raw materials that react chemically are cross-linked to form a stable and firm hybrid network structure. The flame retardant and modified filler can also be evenly dispersed and stably present in the cable material, giving full play to the role of flame retardancy, anti-aging, and enhanced mechanical properties.

[0027] Furthermore, the acrylic acid ester is one or more of methyl acrylate, ethyl acrylate, 2-methyl methacrylate, and 2-ethyl methacrylate.

[0028] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant 1035, and antioxidant 1076.

[0029] Furthermore, the ultraviolet absorber is one or more of ultraviolet absorber UV-531, ultraviolet absorber UVP-327, light stabilizer GW-540, and light stabilizer 744.

[0030] Furthermore, the lubricant is one or more of ethylene bisstearamide, stearic acid, polyethylene wax, and calcium stearate.

[0031] Furthermore, the initiator is one or more of dicumyl peroxide, di-tert-butyl peroxycumene, and dibenzoyl peroxide.

[0032] The beneficial effects of the present invention are as follows: there is a chemical reaction between the modified filler, the flame retardant and the ethylene-vinyl acetate copolymer, the acrylate and the polyethylene, and a stable and firm hybrid network structure is formed, so that the modified filler and the flame retardant can be fully dispersed in the cable material and play a role for a long time, so that the cable material of the present invention has a long-lasting and excellent flame retardant effect, aging resistance and mechanical properties. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] The specific steps for preparing the modified filler are as follows:

[0036] Under nitrogen protection, 5 g of magnesium hydroxide, 3 g of nano-silicon dioxide, 2 g of nano-titanium dioxide, 3.9 g of DMAP and 180 mL of DMSO were added to a 500 mL three-necked flask, and the mixture was stirred thoroughly until uniformly mixed. Subsequently, 15.5 g of maleic anhydride was slowly added. After the addition was completed, the temperature was raised to 50 ° C. and the reaction was kept warm for 12 hours. After the reaction was completed, centrifugation was performed, and the centrifugal precipitate was washed 3 times with deionized water and then washed 3 times with anhydrous ethanol to obtain a modified filler.

[0037] Example 2

[0038] The specific steps for preparing the modified filler are as follows:

[0039] Under nitrogen protection, 5 g of magnesium hydroxide, 3 g of nano-silicon dioxide, 2 g of nano-titanium dioxide, 4.5 g of DMAP and 180 mL of DMSO were added to a 500 mL three-necked flask, and the mixture was stirred thoroughly until uniformly mixed. Then, 14 g of maleic anhydride was slowly added. After the addition was completed, the temperature was raised to 50 ° C. and the reaction was kept warm for 12 hours. After the reaction was completed, centrifugation was performed, and the centrifugal precipitate was washed 3 times with deionized water and then washed 3 times with anhydrous ethanol to obtain a modified filler.

[0040] Example 3

[0041] The specific steps for preparing the modified filler are as follows:

[0042] Under nitrogen protection, 5 g of magnesium hydroxide, 3 g of nano-silicon dioxide, 2 g of nano-titanium dioxide, 4.5 g of DMAP and 180 mL of DMSO were added to a 500 mL three-necked flask, and the mixture was stirred thoroughly until uniformly mixed. Subsequently, 18 g of maleic anhydride was slowly added. After the addition was completed, the temperature was raised to 50 ° C. The reaction was kept warm for 12 hours. After the reaction was completed, centrifugation was performed, and the centrifugal precipitate was washed 3 times with deionized water and then washed 3 times with anhydrous ethanol to obtain a modified filler.

[0043] Example 4

[0044] The flame retardant is prepared in the following steps:

[0045] S1. Under nitrogen protection, 15.6 mL of flame retardant FRC-2, 7.5 mL of pyridine and 120 mL of tetrahydrofuran dried over anhydrous calcium chloride were placed in a 250 mL dry three-necked flask, stirred evenly, and then 6.9 g of phosphorus oxychloride was slowly added. After the addition was completed, it was placed at 0°C for reaction for 0.5 h. After the reaction was completed, centrifuged, the precipitate was dried, and purified by column chromatography (the eluent was a mixed solvent of benzene and ether, and the volume ratio of benzene and ether was 4:6), and distilled under reduced pressure to obtain intermediate 1;

[0046] S2. Under nitrogen protection, 3.5 mL of 2-methylene-1,3-propanediol, 8.3 mL of triethylamine and 80 mL of DMSO were placed in a 250 mL dry brown three-necked flask, stirred evenly, and then 20.1 g of a mixed solution of intermediate 1 and 40 mL of DMSO were slowly added. After the addition was completed, the mixture was placed at 0°C for reaction for 1 hour. After the reaction was completed, the mixture was centrifuged, the precipitate was dried, and purified by column chromatography (a mixed solvent of benzene and ethyl acetate was selected as the eluent, and the volume ratio of benzene and ethyl acetate was 1:1), and distilled under reduced pressure to obtain intermediate 2;

[0047] S3. Blow nitrogen gas into a 500 mL dry three-necked flask for 30 min to drive away the air in the flask, then add 25.5 g of intermediate 2 and 180 mL of DMF, stir to dissolve, then slowly add 5.9 mL of octadecyltrichlorosilane, keep the system temperature below 20°C, raise the temperature to 30°C after the addition, keep the temperature for 6 h, cool to room temperature after the reaction, centrifuge, dry, purify by column chromatography (a mixed solvent of chloroform and acetone is selected as the eluent, and the volume ratio of chloroform and acetone is 7:3), and distill under reduced pressure to obtain a flame retardant.

[0048] Example 5

[0049] The specific steps for preparing cable materials are as follows:

[0050] 70 parts of ethylene-vinyl acetate copolymer, 30 parts of modified filler prepared in Example 3, 20 parts of high-density polyethylene, 10 parts of ethylene-hexene copolymer, 10 parts of flame retardant prepared in Example 4, 5 parts of methyl acrylate, 0.5 parts of antioxidant 1010, 0.5 parts of ultraviolet absorber UV-531, 0.5 parts of calcium stearate and 0.5 parts of diisopropylbenzene peroxide were weighed by weight, and all the raw materials were put into a high-speed mixer and mixed evenly, and then put into a twin-screw extruder for mixing and granulation to obtain a cable material.

[0051] Example 6

[0052] The specific steps for preparing cable materials are as follows:

[0053] 76 parts of ethylene-vinyl acetate copolymer, 34 parts of modified filler prepared in Example 2, 25 parts of high-density polyethylene, 17 parts of ethylene-octene copolymer, 13 parts of flame retardant prepared in Example 4, 8 parts of ethyl acrylate, 0.7 parts of antioxidant 1035, 0.5 parts of ultraviolet absorber UV-531, 0.1 parts of light stabilizer GW-540, 0.4 parts of stearic acid, 0.4 parts of polyethylene wax and 0.8 parts of dibenzoyl peroxide were weighed by weight, and all the raw materials were put into a high-speed mixer and mixed evenly, and then put into a twin-screw extruder for mixing and granulation to obtain a cable material.

[0054] Example 7

[0055] The specific steps for preparing cable materials are as follows:

[0056] 80 parts of ethylene-vinyl acetate copolymer, 40 parts of modified filler prepared in Example 1, 30 parts of high-density polyethylene, 20 parts of ethylene-propylene copolymer, 15 parts of flame retardant prepared in Example 4, 10 parts of 2-ethyl methacrylate, 0.5 parts of antioxidant 1035, 0.5 parts of antioxidant 1076, 0.8 parts of ultraviolet absorber UVP-327, 0.2 parts of light stabilizer 744, 0.5 parts of ethylene bisstearamide, 0.5 parts of calcium stearate and 1 part of di-tert-butyl peroxyisopropylbenzene were weighed by weight, and all the raw materials were put into a high-speed mixer and mixed evenly, and then put into a twin-screw extruder for mixing and granulation to obtain a cable material.

[0057] Comparative Example 1

[0058] The specific steps for preparing cable materials are as follows:

[0059] The remaining steps remain unchanged, except that the modified filler in Example 7 is replaced by a mixture of magnesium hydroxide, nano-silicon dioxide and nano-titanium dioxide in a mass ratio of 5:3:2 to prepare a cable material.

[0060] Comparative Example 2

[0061] The specific steps for preparing cable materials are as follows:

[0062] The remaining steps remained unchanged, only the flame retardant in Example 7 was replaced by 15 parts of flame retardant FRC-2 to prepare the cable material.

[0063] Comparative Example 3

[0064] The specific steps for preparing cable materials are as follows:

[0065] The remaining steps remain unchanged, the modified filler in Example 7 is replaced by a mixture of magnesium hydroxide, nano-silicon dioxide and nano-titanium dioxide in a mass ratio of 5:3:2, and the flame retardant in Example 7 is replaced by 15 parts of flame retardant FRC-2 to prepare a cable material.

[0066] Performance Testing

[0067] The cable materials prepared in Examples 5-7 and Comparative Examples 1-3 were tested for tensile strength and elongation at break according to GB / T1040.3, and the change rates of tensile strength and elongation at break were tested after hot air aging at 110°C for 240h; the oxygen index was tested according to GB / T2406; and the smoke density was tested according to GB / T8323; the test results of all items are shown in the following table:

[0068]

[0069] It can be seen from the test results in the above table that the cable materials prepared in Examples 5-7 of the present invention have excellent flame retardant properties and mechanical properties, and can be used as bending-resistant jumper cable materials for rail vehicles.

[0070] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0071] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a bending-resistant jumper cable material for a rail vehicle, characterized in that: The following steps are involved: Weigh 70-80 parts of ethylene-vinyl acetate copolymer, 30-40 parts of modified filler, 20-30 parts of high-density polyethylene, 10-20 parts of elastomer, 10-15 parts of flame retardant, 5-10 parts of acrylate, 0.5-1 part of antioxidant, 0.5-1 part of ultraviolet absorber, 0.5-1 part of lubricant and 0.5-1 part of initiator by weight, mix well, put into a twin-screw extruder for mixing and granulation, and obtain a cable material; Wherein, the flame retardant is prepared by the following steps: S1. Put flame retardant FRC-2, pyridine and tetrahydrofuran into a flask under nitrogen protection, stir, add phosphorus oxychloride, react at 0°C for 0.5h, centrifuge, dry, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2. Under nitrogen protection, 2-methylene-1,3-propanediol, triethylamine and DMSO were placed in a flask, stirred, and intermediate 1 and DMSO were added. The mixture was reacted at 0°C for 1 h, centrifuged, dried, purified by column chromatography, and distilled under reduced pressure to obtain intermediate 2. S3, after nitrogen blowing into the flask, add intermediate 2 and DMF, stir, add octadecyltrichlorosilane, react at 30°C for 6h, centrifuge, dry, purify by column chromatography, and distill under reduced pressure to obtain a flame retardant; The modified filler is prepared by the following steps: Under nitrogen protection, an inorganic filler, DMAP and DMSO were added to a flask, stirred, and maleic anhydride was added. The mixture was reacted at 50° C. for 12 h, centrifuged and washed to obtain a modified filler.

2. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The amount ratio of phosphorus oxychloride, flame retardant FRC-2, pyridine and tetrahydrofuran in step S1 is 0.045 mol: 0.093 mol: 7.5 mL: 120 mL; the amount ratio of intermediate 1, 2-methylene-1,3-propanediol, triethylamine and DMSO in step S2 is 0.04 mol: 0.043 mol: 8.3 mL: 120 mL; the amount ratio of intermediate 2, octadecyltrichlorosilane and DMF in step S3 is 0.046 mol: 0.015 mol: 180 mL.

3. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The usage ratio of inorganic filler, maleic anhydride, DMAP and DMSO is 10g:14-18g:3.5-4.5g:180mL.

4. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 3, characterized in that: The inorganic filler is a mixture of magnesium hydroxide, nano silicon dioxide and nano titanium dioxide in a mass ratio of 5:3:

2.

5. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The elastomer is one or more of ethylene-octene copolymer, ethylene-propylene copolymer and ethylene-hexene copolymer.

6. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The acrylic acid ester is one or more of methyl acrylate, ethyl acrylate, 2-methyl methacrylate, and 2-ethyl methacrylate.

7. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 1035, and antioxidant 1076.

8. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The ultraviolet absorber is one or more of the ultraviolet absorber UV-531, the ultraviolet absorber UVP-327, the light stabilizer GW-540, and the light stabilizer 744.

9. The method for preparing a bending-resistant jumper cable material for a railway vehicle according to claim 1, characterized in that: The lubricant is one or more of ethylene bisstearamide, stearic acid, polyethylene wax and calcium stearate.

10. The method for preparing a bending-resistant jumper cable material for railway vehicles according to claim 1, characterized in that: The initiator is one or more of dicumyl peroxide, di-tert-butyl peroxycumene, and dibenzoyl peroxide.

Citation Information

Cited By

  • Low-smoke flame-retardant TPE composite material and preparation method thereof

    CN119220043A

  • A low-smoke flame-retardant TPE composite material and preparation method thereof

    CN119220043B

  • High-strength impact-resistant composite heat-resistant plate and preparation method thereof

    CN119463360A

  • Corrosion-resistant crane cable composite material and preparation method thereof

    CN120059329A