Plastic package surface treating agent for electronic device and preparation method of plastic package surface treating agent
By using metal organic compounds, polyimide and graphene oxide on the plastic sealing surface of electronic devices, the problem of insufficient bonding strength between resin plastic sealing materials and metal substrates is solved, and the bonding strength and oxidation resistance are improved. Performance ensures the stability and high temperature performance of the device.
Patent Information
- Application Number
- CN202411190734.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
The bonding force between resin polymer plastic sealing materials and metal substrates is weak, which causes the plastic sealing layer to fall off or break during packaging, affecting product quality.
Using an electronic device plastic sealing surface treatment agent, containing metal organic compounds, polyimides and graphene oxide, the bonding strength and oxidation resistance of the plastic sealing material to the surface of the metal substrate are enhanced, and Adding stabilizers to prevent components from deteriorating and forming a more stable treatment agent.
Effectively improve the bonding strength, thermal stability and oxidation resistance between the plastic sealing material and the surface of the metal substrate, enhance the reliability and stability of the device, prevent the plastic sealing material from peeling or falling off during use, and maintaining it under high temperature environments. Stable operation.
Smart Images

Figure BDA0005015023950000051 
Figure BDA0005015023950000061 
Figure BDA0005015023950000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of surface treatment technology, and in particular to an electronic device plastic packaging surface treatment agent and a preparation method thereof. Background Art
[0002] Plastic encapsulation is a packaging process that covers chips or electronic devices with plastic encapsulation materials for protection. Plastic encapsulation materials can provide structural and mechanical support for electronic devices, protect electronic devices from environmental damage, and maintain the insulation of circuits. Through plastic encapsulation, chips, devices, and connecting lines that were originally exposed to the outside world are protected by the external plastic encapsulation body, preventing the external environment, especially the humid environment, from invading semiconductor devices, thus avoiding product failure.
[0003] At present, the commonly used plastic encapsulation materials are resin-based polymer plastic encapsulation materials such as epoxy resin. Compared with ceramic packaging and metal packaging, resin-based polymer plastic encapsulation materials have the advantages of small size, light weight, simple structure, convenient process, good chemical corrosion resistance, good electrical insulation performance, high mechanical strength, etc., which are convenient for automated production, can improve packaging efficiency and reduce costs. However, the bonding force between resin-based polymer plastic encapsulation materials and metal substrates (ICs, optoelectronic connectors, etc.) is weak, and the plastic encapsulation layer is easy to fall off or break during packaging, causing packaging failure and affecting product quality. Summary of the invention
[0004] In order to solve the above technical problems, the present application provides an electronic device plastic packaging surface treatment agent and a preparation method thereof.
[0005] In a first aspect, the present application provides an electronic device plastic packaging surface treatment agent, which adopts the following technical solution: An electronic device plastic packaging surface treatment agent, comprising the following components in percentage by weight: Metal organic compound 10-30%, polyimide 5-15%, graphene oxide 1-10%, stabilizer 1-5%, solvent 50-80%.
[0006] By adopting the above technical solution, metal organic compounds, polyimide and graphene oxide are dispersed in a solvent to form a treatment agent, and a stabilizer is added for stabilization treatment. Metal organic compounds and polyamide can enhance the bonding strength and thermal stability between the plastic encapsulation material and the metal lead or chip surface; the addition of graphene oxide can enhance the antioxidant performance between the plastic encapsulation material and the metal lead or chip surface, and improve the reliability and stability of the device. Through the coordinated use of metal oxides, polyimide and graphene oxide, the bonding force of the plastic encapsulation material on the surface of the substrate can be effectively enhanced, and the bonding strength, thermal stability and antioxidant capacity between the plastic encapsulation material and the metal lead or chip surface can be improved, thereby improving the reliability and stability of the plastic encapsulation device. The addition of a stabilizer can further prevent the components in the treatment agent from deteriorating or decomposing, and ensure the stability and service life of the treatment agent.
[0007] Optionally, the metal organic compound includes one or a combination of two of aluminum alkoxide and magnesium alkoxide.
[0008] More preferably, the metal organic compound includes one or more combinations of aluminum triethoxide, aluminum isopropoxide, and magnesium isopropoxide.
[0009] By adopting the above technical scheme, metal alkoxide can react with some components in the plastic packaging material to form a chemical bond, thereby enhancing the bonding strength between the plastic packaging material and the metal substrate surface, preventing the plastic packaging material from peeling off or falling off during use. In addition, metal alkoxide can decompose and release metal oxides under high temperature environment, and these metal oxides can improve the thermal stability and high temperature resistance of the plastic packaging material, so that it can be stably operated for a long time under high temperature environment. Aluminum alkoxide has good thermal stability and chemical stability, can enhance the bonding strength between the plastic packaging material and the metal substrate surface, and is suitable for high temperature and high humidity environment, all with good effect. Magnesium alkoxide has good solubility and dispersibility, can improve the film-forming effect and fluidity of the plastic packaging material while enhancing the bonding performance between the plastic packaging material and the metal substrate, and further promotes the stable attachment of the metal substrate surface of the plastic packaging material.
[0010] Optionally, the stabilizer includes one or more combinations of nano-silicon dioxide, organic acid compounds, and silane coupling agents.
[0011] Further preferably, the stabilizer comprises nano-silica, an organic acid compound and a silane coupling agent, and the mass ratio of the nano-silica, the organic acid compound and the silane coupling agent is 1:(1.25-2.5):(0.85-1.75).
[0012] By adopting the above technical solution, the stabilizer composed of nano-silicon dioxide, organic acid compounds and silane coupling agents has good stability and antioxidant properties. On the one hand, it can prevent some components in the treatment agent from deteriorating or decomposing, ensuring the stability and service life of the treatment agent. On the other hand, the addition of organic acid compounds can further improve the adhesion strength of the plastic encapsulation material on the surface of the metal substrate and enhance the adhesion stability of the plastic encapsulation material.
[0013] Optionally, the organic acid compound includes one or more combinations of 4,4-dihydroxymethyl dibenzoate, 4-hydroxybenzoic acid ethyl ester, and 2,4-dinitrophenol.
[0014] Optionally, the stabilizer is prepared by the following method: nano-silicon dioxide and a silane coupling agent are mixed, and then an organic acid compound is added, the temperature is raised to 80-120° C. and kept warm for 0.5-1 h, and the stabilizer is prepared by cooling to room temperature.
[0015] By adopting the above technical scheme, after the silane coupling agent and nano-silica are mixed, the agglomeration of nano-silica can be avoided during the mixing process, and the dispersibility of nano-silica can be improved. The nano-silica treated with the silane coupling agent is mixed with the organic acid compound, and the dispersion and bonding effects between the components in the stabilizer can be enhanced by heating and heat preservation during the mixing process, thereby improving the stability of the stabilizer itself and the dispersion effect of the components.
[0016] Optionally, the solvent includes one or more combinations of acetone, ethyl acetate and isopropanol.
[0017] By adopting the above technical solution, the above substances are selected as solvents, which have good solubility and volatility, can effectively dissolve various components, and can evaporate quickly after being coated on the surface of electronic devices, without causing adverse effects on the electronic devices.
[0018] In a second aspect, the present application provides a method for preparing a surface treatment agent for plastic packaging of electronic devices, using the following technical solution: A method for preparing an electronic device plastic packaging surface treatment agent comprises the following steps: S1. At room temperature, dissolve the metal organic compound, polyimide and graphene oxide in a solvent and mix them evenly; S2, add stabilizer and mix evenly; S3, heating to 60-80°C and keeping warm for 0.5-1h, cooling to room temperature, and obtaining the electronic device plastic sealing surface treatment agent.
[0019] By adopting the above technical solution, the components are first mixed uniformly at room temperature to obtain a mixture, and then the temperature is raised to a specified temperature for insulation reaction. During the insulation process, further reactions occur between the components in the surface treatment agent to form a more stable treatment agent system.
[0020] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the technical solution of the present application, metal organic compounds, polyimide and graphene oxide are dispersed in a solvent to form a treatment agent, and a stabilizer is added for stabilization treatment. Metal organic compounds and polyamide can enhance the bonding strength and thermal stability between the plastic encapsulation material and the metal lead or chip surface; the addition of graphene oxide can enhance the anti-oxidation performance between the plastic encapsulation material and the metal lead or chip surface, and improve the reliability and stability of the device. Through the coordinated use of metal oxides, polyimide and graphene oxide, the bonding force of the plastic encapsulation material on the surface of the substrate can be effectively enhanced, and the bonding strength, thermal stability and anti-oxidation ability between the plastic encapsulation material and the metal lead or chip surface can be improved, thereby improving the reliability and stability of the plastic encapsulation device.
[0021] 2. The metal organic compound is preferably aluminum alkoxide and magnesium alkoxide. Metal alkoxide can react with some components in the plastic encapsulation material to form chemical bonds, thereby enhancing the bonding strength between the plastic encapsulation material and the surface of the metal substrate, and preventing the plastic encapsulation material from peeling off or falling off during use. Under high temperature conditions, metal alkoxides can decompose and release metal oxides, which can improve the thermal stability and high temperature resistance of the plastic encapsulation material, allowing it to operate stably for a long time under high temperature conditions. Aluminum alkoxide has good thermal stability and chemical stability, can enhance the bonding strength between the plastic encapsulation material and the surface of the metal substrate, and is suitable for high temperature and high humidity environments, and has good effects. Magnesium alkoxide has good solubility and dispersibility. While enhancing the bonding performance between the plastic encapsulation material and the metal substrate, it can improve the film-forming effect and fluidity of the plastic encapsulation material, and further promote the stable adhesion of the metal substrate surface of the plastic encapsulation material.
[0022] 3. The stabilizer composed of nano-silicon dioxide, organic acid compounds and silane coupling agents has good stability and antioxidant properties. On the one hand, it can prevent some components in the treatment agent from deteriorating or decomposing, ensuring the stability and service life of the treatment agent. On the other hand, the addition of organic acid compounds can further improve the adhesion strength of the plastic encapsulation material on the surface of the metal substrate and enhance the adhesion stability of the plastic encapsulation material. DETAILED DESCRIPTION
[0023] The present application is further described in detail below in conjunction with specific examples. It should be noted that, if no specific conditions are specified in the following examples, all are carried out under conventional conditions or conditions recommended by the manufacturer; the raw materials used in the following examples can be obtained from common commercial sources unless otherwise specified.
[0024] Example 1 An electronic device plastic sealing surface treatment agent comprises the following components: 10 wt% of aluminum triethanolate, 15 wt% of polyimide, 1 wt% of graphene oxide, 1 wt% of silane coupling agent (KH-560), and 73 wt% of isopropanol, and the total amount of each component is 1 kg; the specific preparation method is as follows: S1. Add aluminum triethoxide, polyimide and graphene oxide to isopropanol at room temperature and stir to completely dissolve to obtain a mixed solution; S2, adding silane coupling agent to the mixed solution prepared in step S1 and stirring to mix evenly; S3, heating the mixed solution obtained in step S2 to 75° C. and keeping the temperature for 1 hour, and then naturally cooling it to room temperature to obtain a plastic sealing surface treatment agent for electronic devices.
[0025] Example 2 The difference between this embodiment and embodiment 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with embodiment 1.
[0026] Example 3 The difference between this embodiment and embodiment 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with embodiment 1.
[0027] Example 4 The difference between this embodiment and embodiment 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with embodiment 1.
[0028] Comparative Example 1 The difference between this comparative example and Example 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with Example 1.
[0029] Comparative Example 2 The difference between this comparative example and Example 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with Example 1.
[0030] Comparative Example 3 The difference between this comparative example and Example 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with Example 1.
[0031] Comparative Example 4 The difference between this comparative example and Example 1 is that the composition ratio of the raw materials is different, please refer to Table 1 for details, and the rest is consistent with Example 1.
[0032] Table 1: Examples 2-4 Raw material composition ratio (wt%) Metal organic compounds Polyimide Graphene oxide Stabilizer Solvents Example 2 30 5 10 5 50 Example 3 15 12 5 3 65 Example 4 22 8 6 2 62 Comparative Example 1 5 5 10 5 75 Comparative Example 2 30 1 10 5 54 Comparative Example 3 30 5 0 5 60 Comparative Example 4 30 5 10 0 55 Performance test and stability test: Take the evenly mixed surface treatment agent and let it stand for 144 hours to observe whether there is any stratification, precipitation, agglomeration, discoloration, etc.
[0033] Copper sheets and silver-plated copper sheets were soaked in the plastic surface treatment agents for electronic devices prepared in the above embodiments and comparative examples, taken out and dried at room temperature, and then epoxy resin plastic molding material (Sumitomo Bakelite, model: EME-G600) was used to plastic mold the surface of the sample, and then the performance was tested. The test items are as follows: Adhesion: A shear force is applied along the surface of the sample at a speed of 20 mm / min to test the maximum force value before the plastic encapsulation material is separated from the sample. Five groups are tested for each embodiment and the average value is taken (except for outliers). A control group is also set up, which is not treated with a surface treatment agent and the adhesion of the plastic encapsulation material is tested.
[0034] Thermal conductivity: After the plastic encapsulation material is coated on the sample and cured, its thermal conductivity is tested according to ASTM D5470-2012.
[0035] The performance test results of Examples 1-4 and Comparative Examples 1-4 are shown in Table 2 below.
[0036] Table 2: Performance test results of Examples 1-4 and Comparative Examples 1-4 From the data in Table 2, it can be seen that after being treated with the surface treatment agent, the adhesion strength of the epoxy resin molding compound on the copper surface and the silver surface is significantly improved, and the bonding force is significantly enhanced. Compared with the metal substrate surface not treated with the surface treatment agent, the bonding force of the epoxy resin molding compound is greatly improved.
[0037] It can be seen from the data of Comparative Examples 3 and 4 that the addition of graphene oxide and stabilizer can improve the stability of the surface treatment agent itself, and can exist stably under long-term storage without deterioration or decomposition.
[0038] Example 5 The difference between this embodiment and embodiment 4 is that an equal amount of magnesium isopropoxide is used instead of aluminum triethoxide, and the rest is consistent with embodiment 1.
[0039] Example 6 The difference between this embodiment and embodiment 4 is that a mixture of equal amounts of aluminum isopropoxide and magnesium isopropoxide is used instead of aluminum triethoxide, the mass ratio of aluminum isopropoxide to magnesium isopropoxide is 1:1, and the rest is consistent with embodiment 4.
[0040] Example 7 The difference between this embodiment and embodiment 4 is that the stabilizer comprises nano-silicon dioxide, an organic acid compound and a silane coupling agent, the mass ratio of the nano-silicon dioxide, the organic acid compound and the silane coupling agent is 1:1:1, the organic acid compound is ethyl 4-hydroxybenzoate, and the stabilizer is prepared by the following method: Nano-silica and silane coupling agent were mixed and stirred to be uniformly dispersed, and then ethyl 4-hydroxybenzoate was added and continued to be stirred and mixed uniformly, and then the temperature was raised to 90° C., the reaction was kept at this temperature for 1 hour, and the stabilizer was naturally cooled to room temperature to obtain the stabilizer.
[0041] The rest are consistent with Example 4.
[0042] Example 8 The difference between this embodiment and embodiment 7 is that the mass ratio of nano-silicon dioxide, organic acid compound and silane coupling agent is 1:2:1, and the rest is consistent with embodiment 7.
[0043] Example 9 The difference between this embodiment and embodiment 7 is that the mass ratio of nano-silicon dioxide, organic acid compound and silane coupling agent is 1:1.5:1.5, and the rest is consistent with embodiment 7.
[0044] Example 10 The difference between this embodiment and embodiment 7 is that the mass ratio of nano-silicon dioxide, organic acid compound and silane coupling agent is 2:1:1.5, and the rest is consistent with embodiment 7.
[0045] Embodiment 11 The difference between this embodiment and embodiment 7 is that an equal amount of 2,4-dinitrophenol is used instead of ethyl 4-hydroxybenzoate, and the rest is consistent with embodiment 7.
[0046] Example 12 The difference between this embodiment and embodiment 7 is that an equal amount of a mixture of 2,4-dinitrophenol and ethyl 4-hydroxybenzoate is used instead of ethyl 4-hydroxybenzoate, the mass ratio of 2,4-dinitrophenol to ethyl 4-hydroxybenzoate is 1:2, and the rest is consistent with embodiment 7.
[0047] Embodiment 13 The difference between this embodiment and embodiment 7 is that the stabilizer is prepared by the following method: Nano-silicon dioxide and a silane coupling agent are mixed and stirred to be uniformly dispersed, and then ethyl 4-hydroxybenzoate is added and continued to be stirred and mixed to obtain a stabilizer.
[0048] The rest are consistent with Example 7.
[0049] The performance test results of Examples 5-13 are shown in Table 3 below.
[0050] Table 2: Performance test results of Examples 5-13 It can be seen from the data in Table 3 that the specific composition ratio of metal organic compound and stabilizer will also affect the stability of surface treatment agent and the surface treatment effect on metal substrate. Specifically, it can be seen from the performance test data of Examples 4-6 that the combination of aluminum isopropoxide and magnesium isopropoxide is added as metal organic compound, which can further improve the performance of surface treatment machine, and epoxy resin molding compound has a better bonding effect on the metal substrate surface, which may be because aluminum alkoxide has good thermal stability and chemical stability, can enhance the bonding strength between molding material and metal substrate surface, and is suitable for high temperature and high humidity environment, all with good effect; magnesium alkoxide has good solubility and dispersibility, can enhance the film-forming effect and fluidity of molding material while enhancing the bonding performance between molding material and metal substrate, further promote the stable attachment of the metal substrate surface of molding material, and the mutual coordination of aluminum alkoxide and magnesium alkoxide makes the performance of surface treatment agent better.
[0051] It can be seen from the performance test data of Examples 7-10 that the performance of the surface treatment obtained by adding nano-silica, organic acid compounds and silane coupling agents as stabilizers in a specific combination ratio will be further improved. This may be because the three of nano-silica, organic acid compounds and silane coupling agents cooperate with each other, which on the one hand further improves the stability of the surface treatment machine itself, and on the other hand improves the fluidity of the surface treatment agent and the film-forming performance on the surface of the metal substrate, thereby having better surface treatment capabilities.
[0052] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. An electronic device plastic packaging surface treatment agent, characterized in that: The invention comprises the following components in weight percentage: 10-30% of metal organic compound, 5-15% of polyimide, 1-10% of graphene oxide, 1-5% of stabilizer and 50-80% of solvent.
2. The surface treatment agent for plastic packaging of electronic devices according to claim 1, characterized in that: The metal organic compound includes one or a combination of aluminum alkoxide and magnesium alkoxide.
3. The surface treatment agent for plastic packaging of electronic devices according to claim 2, characterized in that: The metal organic compound includes one or more combinations of aluminum triethoxide, aluminum isopropoxide, and magnesium isopropoxide.
4. The surface treatment agent for plastic packaging of electronic devices according to claim 1, characterized in that: The stabilizer includes one or more combinations of nano silicon dioxide, organic acid compounds, and silane coupling agents.
5. The surface treatment agent for plastic packaging of electronic devices according to claim 4, characterized in that: The stabilizer comprises nano silicon dioxide, an organic acid compound and a silane coupling agent, and the mass ratio of the nano silicon dioxide, the organic acid compound and the silane coupling agent is 1:(1.25-2.5):(0.85-1.75).
6. The surface treatment agent for plastic packaging of electronic devices according to claim 5, characterized in that: The stabilizer is prepared by the following method: nano silicon dioxide and a silane coupling agent are mixed, then an organic acid compound is added, the temperature is raised to 80-120° C. and kept for 0.5-1 h, and the stabilizer is prepared by cooling to room temperature.
7. The surface treatment agent for plastic packaging of electronic devices according to claim 4, characterized in that: The organic acid compound includes one or more combinations of 4,4-dihydroxymethyl dibenzoic acid diester, 4-hydroxybenzoic acid ethyl ester, and 2,4-dinitrophenol.
8. The surface treatment agent for plastic packaging of electronic devices according to claim 7, characterized in that: The solvent includes one or more combinations of acetone, ethyl acetate and isopropanol.
9. The method for preparing a surface treatment agent for plastic packaging of electronic devices according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. At room temperature, dissolve the metal organic compound, polyimide and graphene oxide in a solvent and mix them evenly; S2, add stabilizer and mix evenly; S3, heating to 60-80°C and keeping warm for 0.5-1h, cooling to room temperature, and obtaining the electronic device plastic sealing surface treatment agent.
Citation Information
Patent Citations
Heat-resistant high-light-transmitting modified epoxy resin adhesive applied to chip encapsulation of LED plant growth lamp
CN106085322A
High temperature resistant polyamide-imide nano ultrathin membrane, and preparation method thereof
CN106497053A
Surface treatment of inorganic particle
JP1998036705A
Flexible display device
KR1020220043560A
Graphene Oxide-Filled Polyimide Films and Process
US20210125741A1
Cited By
Chip protection film with anti-reflection function and preparation method thereof
CN120399566A