Tubular liquid two-component filling silica gel and use method thereof

By using instant mixing technology of tube-mounted liquid two-component filled silicone in sealing materials, the problems of long curing time and insufficient performance of existing sealing materials are solved, and rapid curing and high-performance sealing effect is achieved, and construction efficiency is improved. Scope of application.

CN118931489AInactive Publication Date: 2024-11-12FUJIAN ZHIWEI NEW MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411256445.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing sealing materials have a long curing time and are inadequate in flame retardant, waterproof and shock-absorbing performance, which is difficult to meet in applications where rapid curing and high performance requirements are required.

Method used

Provide a tube-filled liquid two-component filled silicone, which is mixed in proportion by component A and component B, and includes methyl ethylene silicone rubber, polymer, foaming agent, crosslinking agent, catalyst and flame retardant powder. As well as isocyanate, hydrogen-containing silicone oil and curing agent, use a two-component glue gun and a static stirring mixing head for instant mixing to ensure construction efficiency and performance.

Benefits of technology

It achieves the effects of short curing time, high viscosity, high temperature resistance, electrical insulation, oxidation stability, high flame retardant performance, waterproof, corrosion resistance and environmental protection and non-toxicity, improves construction efficiency and product application scope, and reduces costs and Waste of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931489A_ABST
    Figure CN118931489A_ABST
Patent Text Reader

Abstract

The invention discloses tubing liquid two-component filling silica gel and a use method, the tubing liquid two-component filling silica gel is prepared by filling a component A and a component B into a tube body A and a tube body B of a two-component tube in proportion, and the component A comprises the following raw materials: methyl vinyl silicone rubber, a cross-linking agent, a catalyst and flame-retardant powder; and the component B comprises the following raw materials: isocyanate, hydrogen-containing silicone oil and a curing agent. The tubing liquid two-component filling silica gel provided by the invention has the advantages of short curing time, high waterproof and flame-retardant grade, filling shock absorption, no toxicity and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing filling materials, and in particular to a tube-packed liquid two-component filling silica gel and a use method thereof. Background Art

[0002] Among the existing sealing materials, traditional one-component silicone and two-component polyurethane foam sealants are two common choices. They do show certain effects in terms of waterproofing, flame retardancy, shock absorption, etc., but they also have some obvious shortcomings.

[0003] Although one-component silicone is easy to use, its curing time is relatively long, which affects the construction efficiency to a certain extent. At the same time, it also has certain limitations in flame retardant performance and may not meet certain application scenarios with high fire protection requirements.

[0004] Two-component polyurethane foam sealant has significant advantages in thermal insulation performance and material strength, which makes it perform well in some occasions that require thermal insulation and support. However, its curing time is also relatively long, which often delays the construction progress and reduces the overall construction efficiency. In addition, although the thermal insulation performance of two-component polyurethane foam sealant is excellent, it still needs to be improved in terms of waterproofing, flame retardancy, shock absorption, and environmental protection, especially in some specific applications that require fast curing and high performance.

[0005] Therefore, there is an urgent need for a two-component filled silicone that can cure quickly, is waterproof and flame retardant, shock-absorbing, and is environmentally friendly and non-toxic. Summary of the invention

[0006] In order to overcome the problems of slow curing time, insufficient waterproof and flame retardant and shock absorbing performance of existing sealing materials, the present invention provides a tube-packed liquid two-component filling silicone and a use method, which has the advantages of short curing time, high waterproof and flame retardant grade, filling shock absorption, non-toxic and environmentally friendly.

[0007] The technical solution of the present invention is as follows:

[0008] In a first aspect, the present invention provides a tube-packed liquid two-component silica gel, which is prepared by filling component A and component B into the A and B tube bodies of the two-component tube in proportion.

[0009] The raw materials of component A include: methyl vinyl silicone rubber, high molecular polymer, foaming agent, cross-linking agent, catalyst and flame retardant powder;

[0010] The raw materials of component B include: isocyanate, hydrogen-containing silicone oil and curing agent.

[0011] As a preferred embodiment of the present invention, the mass ratio of the component A to the component B is 1:1.

[0012] As a preferred embodiment of the present invention, the mass percentage ratio of each raw material in the component A is:

[0013] Methyl vinyl silicone rubber: 20-40%;

[0014] High molecular weight polymer: 10-20%;

[0015] Foaming agent: 15-30%;

[0016] Cross-linking agent: 5-10%;

[0017] Catalyst: 5-10%;

[0018] Flame retardant powder: 20~40%.

[0019] As a preferred embodiment of the present invention, the mass percentage ratio of each raw material in the B component is:

[0020] Isocyanate: 50-70%;

[0021] Hydrogenated silicone oil: 20-40%;

[0022] Curing agent: 10~30%.

[0023] As a preferred embodiment of the present invention, the high molecular polymer is polyurethane or TPU prepolymer.

[0024] As a preferred embodiment of the present invention, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymeric MDI I.

[0025] As a preferred embodiment of the present invention, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.

[0026] As a preferred embodiment of the present invention, the curing agent is a platinum catalyst.

[0027] As a preferred embodiment of the present invention, the preparation method of component A comprises:

[0028] The methyl vinyl silicone rubber and the high molecular polymer are put into a reactor according to a ratio for premixing. After premixing for 5 to 8 hours, the flame retardant powder, the foaming agent, the catalyst and the crosslinking agent are added in sequence according to the components and mixed for 1 to 2 hours. The rotation speed of the reactor is 100 to 120 r / min. After the premixing, the rotation speed of the reactor is 160 to 190 r / min.

[0029] As a preferred embodiment of the present invention, the preparation method of component B comprises:

[0030] The isocyanate, the cross-linking agent and the curing agent are placed in a reaction kettle according to a ratio and mixed for 2 to 4 hours. The rotation speed of the reaction kettle is 200 to 230 r / min.

[0031] In a second aspect, the present invention provides a method for using the tube-packed liquid two-component filling silica gel as described in any of the above schemes, comprising the following steps:

[0032] Remove the front end plug of the tube-packed liquid two-component silicone filling and install the matching static stirring mixing tube head;

[0033] Install the tube-type liquid two-component filling silicone equipped with a static stirring mixing tube head onto the two-component glue gun;

[0034] When the trigger of the two-component glue gun is pulled, the push rod of the two-component glue gun pushes the A and B components of the tube-filled liquid two-component filling silicone to flow out synchronously to the static stirring mixing tube head for mixing. As the push rod continues to advance, the fully mixed filling silicone is output from the output port of the static stirring mixing tube head.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. By controlling the pre-reaction of component A and the raw material ratio and reaction conditions of each raw material in component A and component B, the prepared tubular liquid two-component filling silicone has a variety of superior properties, including short curing time, high viscosity, high and low temperature resistance, electrical insulation, oxidation stability, weather resistance, high flame retardancy, waterproof, corrosion resistance, non-toxic and environmentally friendly, etc., which effectively improves construction efficiency, reduces production costs, and expands the scope of application of the product;

[0037] 2. By using a two-component glue gun and a static stirring and mixing tube head, the A and B components of the tube-packed liquid two-component silicone filling can be quickly and evenly mixed during the outflow process. This instant mixing method ensures that the filling silicone is completely mixed when it reaches the application site, avoiding the unevenness and time consumption that may be caused by manual mixing. The entire use process is simple and fast. You only need to install the tube-packed silicone on the two-component glue gun and pull the trigger to start construction, which greatly improves construction efficiency and reduces the operating difficulty and labor intensity of construction personnel. At the same time, since the mixing process is completed in the static stirring and mixing tube head, and it is immediately mixed and used, the waste and pollution of materials during the mixing process are reduced. In addition, the tube-packed design is also convenient for storage and transportation, further reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 It is a structural schematic diagram of a tube-packed liquid two-component filling silicone being installed in a two-component glue gun in one embodiment of the present invention;

[0040] Figure 2 Schematic diagram of the structure of a tube-packed liquid two-component filling silica gel in one embodiment of the present invention. DETAILED DESCRIPTION

[0041] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. It is also stated that the embodiments described below are only used to explain the present invention and are not used to limit the present invention.

[0042] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device including a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.

[0043] Example 1

[0044] The invention provides a tubular liquid two-component filling silica gel, which is prepared by filling component A and component B into A and B tube bodies of a two-component tube at a mass ratio of 1:1.

[0045] Among them, the mass percentage ratio of each raw material in component A is:

[0046] Methyl vinyl silicone rubber: 30%;

[0047] High molecular weight polymer: 15%;

[0048] Foaming agent: 25%;

[0049] Cross-linking agent: 5%;

[0050] Catalyst: 5%;

[0051] Flame retardant powder: 20%.

[0052] Among them, the mass percentage ratio of each raw material in component B is:

[0053] Isocyanate: 60%;

[0054] Hydrogenated silicone oil: 25%;

[0055] Curing agent: 15%.

[0056] The preparation method of component A is as follows: put methyl vinyl silicone rubber and high molecular polymer into a reactor for premixing according to the ratio, add flame retardant powder, foaming agent, catalyst and crosslinking agent in order according to the components for 8 hours, and mix for 2 hours. The speed of the reactor is 100r / min. After the premixing, the speed of the reactor is 160r / min. The crosslinking agent is used to promote the chemical reaction of the foaming agent to produce more gas, thereby increasing the volume and stability of the filled silica gel, and can also enhance the temperature resistance and mechanical strength of the filled silica gel.

[0057] The preparation method of component B is as follows: isocyanate, cross-linking agent and curing agent are put into a reaction kettle according to a ratio and mixed for 4 hours, and the rotation speed of the reaction kettle is 200 r / min.

[0058] Furthermore, the high molecular polymer is polyurethane. Polyurethane is a new type of high molecular synthetic material between rubber and plastic. It combines the high strength of plastic and the high elasticity of rubber, and has the characteristics of high hardness and high resilience. The present invention adds polyurethane to component A in a certain proportion, and adjusts the amount of foaming agent, cross-linking agent and catalyst to ensure good compatibility with the newly added polyurethane and maintain appropriate foaming and cross-linking speeds, thereby improving the elasticity and shock absorption performance of the tube-filled liquid two-component filling silicone rubber to meet higher requirements for sealing and shock absorption applications.

[0059] Furthermore, the isocyanate is toluene diisocyanate.

[0060] Furthermore, the flame retardant powder is one of aluminum hydroxide and magnesium hydroxide.

[0061] Furthermore, the curing agent is a platinum catalyst. Platinum catalysts have high catalytic activity and can efficiently promote cross-linking reactions between silicone polymers. The silicon-oxygen bonds formed by platinum catalysts are very stable, which helps to improve the temperature resistance, chemical resistance and weather resistance of the final product. Compared with other types of catalysts, platinum catalysts have lower toxicity, which makes them very useful in industries that need to meet strict safety and health standards. Platinum catalysts have less effect on the color and odor of the cured product, which is especially important for products that require transparency or specific color requirements. Platinum catalysts can improve the mechanical properties of silicone, such as hardness and elasticity, while maintaining the flexibility of the material.

[0062] Example 2

[0063] The invention provides a tubular liquid two-component filling silica gel, which is prepared by filling component A and component B into A and B tube bodies of a two-component tube at a mass ratio of 1:1.

[0064] Among them, the mass percentage ratio of each raw material in component A is:

[0065] Methyl vinyl silicone rubber: 20%;

[0066] High molecular weight polymer: 10%;

[0067] Foaming agent: 30%;

[0068] Cross-linking agent: 5%;

[0069] Catalyst: 5%;

[0070] Flame retardant powder: 40%.

[0071] Among them, the mass percentage ratio of each raw material in component B is:

[0072] Isocyanate: 50%;

[0073] Hydrogenated silicone oil: 20%;

[0074] Curing agent: 30%.

[0075] The preparation method of component A is as follows: put methyl vinyl silicone rubber and high molecular polymer into a reactor for premixing according to the ratio, add flame retardant powder, foaming agent, catalyst and crosslinking agent in order according to the components for 5 hours, and mix for 1 hour. The speed of the reactor is 120r / min. After the premixing, the speed of the reactor is 190r / min. The crosslinking agent is used to promote the chemical reaction of the foaming agent to produce more gas, thereby increasing the volume and stability of the filled silica gel, and can also enhance the temperature resistance and mechanical strength of the filled silica gel.

[0076] The preparation method of component B is as follows: isocyanate, cross-linking agent and curing agent are put into a reaction kettle according to a ratio and mixed for 2 hours, and the rotation speed of the reaction kettle is 230 r / min.

[0077] Furthermore, the high molecular polymer is TPU (Thermoplastic Polyurethane) prepolymer, which is a non-toxic and environmentally friendly high molecular polymer with a wide hardness range, high mechanical strength, outstanding impact resistance and shock absorption performance, and also exhibits excellent electrical insulation, high and low temperature resistance, oxidation stability, weather resistance, corrosion resistance and other properties. The present invention adds TPU prepolymer to component A in a certain proportion, and adjusts the amount of foaming agent, cross-linking agent and catalyst to ensure good compatibility with the newly added TPU prepolymer and maintain appropriate foaming and cross-linking speeds, which can not only improve the elasticity and shock absorption performance of the tube-packed liquid two-component filling silicone, but also improve the product's electrical insulation, high and low temperature resistance, oxidation stability, weather resistance, corrosion resistance, and maintain the product's environmental characteristics.

[0078] Furthermore, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.

[0079] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.

[0080] Furthermore, the curing agent is a platinum catalyst. Platinum catalysts have high catalytic activity and can efficiently promote cross-linking reactions between silicone polymers. The silicon-oxygen bonds formed by platinum catalysts are very stable, which helps to improve the temperature resistance, chemical resistance and weather resistance of the final product. Compared with other types of catalysts, platinum catalysts have lower toxicity, which makes them very useful in industries that need to meet strict safety and health standards. Platinum catalysts have less effect on the color and odor of the cured product, which is especially important for products that require transparency or specific color requirements. Platinum catalysts can improve the mechanical properties of silicone, such as hardness and elasticity, while maintaining the flexibility of the material.

[0081] Example 3

[0082] The invention provides a tubular liquid two-component filling silica gel, which is prepared by filling component A and component B into A and B tube bodies of a two-component tube at a mass ratio of 1:1.

[0083] Among them, the mass percentage ratio of each raw material in component A is:

[0084] Methyl vinyl silicone rubber: 30%;

[0085] High molecular weight polymer: 15%;

[0086] Foaming agent: 20%;

[0087] Cross-linking agent: 10%;

[0088] Catalyst: 5%;

[0089] Flame retardant powder: 20%.

[0090] Among them, the mass percentage ratio of each raw material in component B is:

[0091] Isocyanate: 50%;

[0092] Hydrogenated silicone oil: 40%;

[0093] Curing agent: 10%.

[0094] The preparation method of component A is as follows: put methylvinyl silicone rubber and high molecular polymer into a reactor for premixing according to the ratio, add flame retardant powder, foaming agent, catalyst and crosslinking agent in order according to the components for 7 hours, and mix for 2 hours. The speed of the reactor is 110r / min, and the speed of the reactor is 170r / min after the premixing. The crosslinking agent is used to promote the chemical reaction of the foaming agent to produce more gas, thereby increasing the volume and stability of the filled silica gel, and can also enhance the temperature resistance and mechanical strength of the filled silica gel.

[0095] The preparation method of component B is as follows: isocyanate, cross-linking agent and curing agent are put into a reaction kettle according to a ratio and mixed for 2 hours, and the rotation speed of the reaction kettle is 200 r / min.

[0096] Furthermore, the high molecular polymer is polyurethane. Polyurethane is a new type of high molecular synthetic material between rubber and plastic. It combines the high strength of plastic and the high elasticity of rubber, and has the characteristics of high hardness and high resilience. The present invention adds polyurethane to component A in a certain proportion, and adjusts the amount of foaming agent, cross-linking agent and catalyst to ensure good compatibility with the newly added polyurethane and maintain appropriate foaming and cross-linking speeds, thereby improving the elasticity and shock absorption performance of the tube-filled liquid two-component filling silicone rubber to meet higher requirements for sealing and shock absorption applications.

[0097] Furthermore, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.

[0098] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.

[0099] Furthermore, the curing agent is a platinum catalyst. Platinum catalysts have high catalytic activity and can efficiently promote cross-linking reactions between silicone polymers. The silicon-oxygen bonds formed by platinum catalysts are very stable, which helps to improve the temperature resistance, chemical resistance and weather resistance of the final product. Compared with other types of catalysts, platinum catalysts have lower toxicity, which makes them very useful in industries that need to meet strict safety and health standards. Platinum catalysts have less effect on the color and odor of the cured product, which is especially important for products that require transparency or specific color requirements. Platinum catalysts can improve the mechanical properties of silicone, such as hardness and elasticity, while maintaining the flexibility of the material.

[0100] Example 4

[0101] The invention provides a tubular liquid two-component filling silica gel, which is prepared by filling component A and component B into A and B tube bodies of a two-component tube at a mass ratio of 1:1.

[0102] Among them, the mass percentage ratio of each raw material in component A is:

[0103] Methyl vinyl silicone rubber: 40%;

[0104] High molecular weight polymer: 10%;

[0105] Foaming agent: 15%;

[0106] Cross-linking agent: 5%;

[0107] Catalyst: 10%;

[0108] Flame retardant powder: 20%.

[0109] Among them, the mass percentage ratio of each raw material in component B is:

[0110] Isocyanate: 60%;

[0111] Hydrogenated silicone oil: 30%;

[0112] Curing agent: 10%.

[0113] The preparation method of component A is as follows: put methyl vinyl silicone rubber and high molecular polymer into a reactor according to the ratio for premixing, add flame retardant powder, foaming agent, catalyst and crosslinking agent in order according to the components for 8 hours, and mix for 1 hour. The speed of the reactor is 100r / min. After the premixing, the speed of the reactor is 190r / min. The crosslinking agent is used to promote the chemical reaction of the foaming agent to produce more gas, thereby increasing the volume and stability of the filled silica gel, and can also enhance the temperature resistance and mechanical strength of the filled silica gel.

[0114] The preparation method of component B is as follows: isocyanate, crosslinking agent and curing agent are put into a reactor according to the ratio and mixed for 3 hours, and the speed of the reactor is 200r / min.

[0115] Furthermore, the high molecular polymer is a TPU prepolymer. TPU prepolymer is a non-toxic and environmentally friendly high molecular polymer with the characteristics of a wide hardness range, high mechanical strength, outstanding impact resistance and shock absorption performance, and also exhibits excellent electrical insulation, high and low temperature resistance, oxidation stability, weather resistance, corrosion resistance and other properties. The present invention adds TPU prepolymer to component A in a certain proportion, and adjusts the amount of foaming agent, cross-linking agent and catalyst to ensure good compatibility with the newly added TPU prepolymer and maintain appropriate foaming and cross-linking speeds, which can not only improve the elasticity and shock absorption performance of the tube-packed liquid two-component filling silicone, but also improve the product's electrical insulation, high and low temperature resistance, oxidation stability, weather resistance, corrosion resistance, and maintain the product's environmental characteristics.

[0116] Furthermore, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.

[0117] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.

[0118] Furthermore, the curing agent is a platinum catalyst. Platinum catalysts have high catalytic activity and can efficiently promote cross-linking reactions between silicone polymers. The silicon-oxygen bonds formed by platinum catalysts are very stable, which helps to improve the temperature resistance, chemical resistance and weather resistance of the final product. Compared with other types of catalysts, platinum catalysts have lower toxicity, which makes them very useful in industries that need to meet strict safety and health standards. Platinum catalysts have less effect on the color and odor of the cured product, which is especially important for products that require transparency or specific color requirements. Platinum catalysts can improve the mechanical properties of silicone, such as hardness and elasticity, while maintaining the flexibility of the material.

[0119] Example 5

[0120] See also Figure 1 , Figure 2 The present invention provides a method for using a tube-packed liquid two-component filling silica gel, comprising the following steps:

[0121] Remove the front end plug 2 of the tube-packed liquid two-component filling silica gel 1 described in any of the above embodiments, and install the matching static stirring mixing tube head 3;

[0122] Install the tube-type liquid two-component filling silicone 1 equipped with a static stirring mixing tube head 3 onto a two-component glue gun 4;

[0123] By pulling the trigger of the two-component glue gun 4, the push rod 41 of the two-component glue gun 4 pushes the A and B components of the tube-filled liquid two-component filling silicone 1 to flow out synchronously into the static stirring mixing tube head 3 for mixing. As the push rod 41 continues to advance, the fully mixed filling silicone is output from the output port of the static stirring mixing tube head 3.

[0124] The present invention uses a two-component glue gun and a static stirring mixing tube head in combination, so that the A and B components of the tube-packaged liquid two-component filling silicone can be quickly and evenly mixed during the outflow process. This instant mixing method ensures that the filling silicone is in a completely mixed state when it reaches the application site, avoiding the unevenness and time consumption that may be caused by manual mixing; the entire use process is simple and fast, and only needs to install the tube-packaged silicone on the two-component glue gun and hook the trigger to start construction, which greatly improves construction efficiency and reduces the operating difficulty and labor intensity of construction personnel; at the same time, because the mixing process is completed in the static stirring mixing tube head, and it is instant mixing and instant use, the waste and pollution of materials in the mixing process are reduced; in addition, the tube-packaged design is also convenient for storage and transportation, further reducing costs.

[0125] Test case performance test

[0126] The performance of the tubular liquid two-component filling silicone prepared in Examples 1-4 of the present invention was compared with the existing one-component silicone and two-component polyurethane foam sealant. The results are shown in Table 1.

[0127] Table 1 Performance test results

[0128]

[0129] It can be seen from the above table that the tubular liquid two-component filling silicone prepared in Examples 1-4 of the present invention has the advantages of short curing time, high viscosity, high and low temperature resistance, electrical insulation, oxidation stability, weather resistance, high flame retardancy, waterproofness, corrosion resistance, etc., compared with the existing one-component silicone and two-component polyurethane foam sealant, which effectively improves the construction efficiency, reduces the production cost, and expands the application range of the product.

[0130] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.

[0131] The above is an exemplary description of the present invention. Obviously, the implementation of the present invention is not limited to the above method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A tube-packed liquid two-component silica gel, which is made by filling component A and component B into the A and B tube bodies of the two-component tube in proportion, characterized in that: The raw materials of component A include: methyl vinyl silicone rubber, high molecular polymer, foaming agent, cross-linking agent, catalyst and flame retardant powder; The raw materials of component B include: isocyanate, hydrogen-containing silicone oil and curing agent.

2. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The mass ratio of the component A to the component B is 1:

1.

3. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The mass percentage ratio of each raw material in the A component is: Methyl vinyl silicone rubber: 20-40%; High molecular weight polymer: 10-20%; Foaming agent: 15-30%; Cross-linking agent: 5-10%; Catalyst: 5-10%; Flame retardant powder: 20~40%.

4. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The mass percentage ratio of each raw material in the B component is: Isocyanate: 50-70%; Hydrogenated silicone oil: 20-40%; Curing agent: 10~30%.

5. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The high molecular polymer is polyurethane or TPU prepolymer.

6. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.

7. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The curing agent is a platinum catalyst.

8. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The preparation method of component A comprises: The methyl vinyl silicone rubber and the high molecular polymer are put into a reactor according to a ratio for premixing. After premixing for 5 to 8 hours, the flame retardant powder, the foaming agent, the catalyst and the crosslinking agent are added in sequence according to the components and mixed for 1 to 2 hours. The rotation speed of the reactor is 100 to 120 r / min. After the premixing, the rotation speed of the reactor is 160 to 190 r / min.

9. The tube-packed liquid two-component filling silica gel according to claim 1, characterized in that: The preparation method of the component B comprises: The isocyanate, the cross-linking agent and the curing agent are placed in a reaction kettle according to a ratio and mixed for 2 to 4 hours. The rotation speed of the reaction kettle is 200 to 230 r / min.

10. A method for using the tube-packed liquid two-component filling silica gel according to any one of claims 1 to 9, characterized in that: The following steps are involved: Remove the front end plug of the tube-packed liquid two-component silicone filling and install the matching static stirring mixing tube head; Install the tube-type liquid two-component filling silicone equipped with a static stirring mixing tube head onto the two-component glue gun; When the trigger of the two-component glue gun is pulled, the push rod of the two-component glue gun pushes the A and B components of the tube-filled liquid two-component filling silicone to flow out synchronously to the static stirring mixing tube head for mixing. As the push rod continues to advance, the fully mixed filling silicone is output from the output port of the static stirring mixing tube head.

Citation Information

Patent Citations

  • Polyurethane / silicon rubber thermoplastic elastomer and preparation method thereof

    CN102153853A

  • Silicon rubber for encapsulating electronic tube and encapsulating method

    CN102964839A

  • Two-component polyurethane adhesive for grinding tool and preparation method of two-component polyurethane adhesive

    CN106674483A

  • Flame-retardant thermoplastic dynamic silicon-sulfide rubber and preparation method thereof

    CN109593349A

  • Method for preparing organic silicon thermoplastic vulcanized rubber by double-premixing dynamic vulcanization process