Porous magnesium alloy with high electromagnetic shielding effectiveness and preparation method
Through the Gasar directional solidification process of Mg-Ag-Sn-based porous magnesium alloy, a material with high electromagnetic shielding performance was prepared, which solved the shortcomings of existing electromagnetic shielding materials in high bands and lightweight, and achieved thin, light, The characteristics of wide and strong enhance the electromagnetic wave energy reduction ability and material strength.
Patent Information
- Application Number
- CN202411015155.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing electromagnetic shielding materials have shortcomings in meeting the requirements of high-band electromagnetic shielding, lightweight and structural strength. Traditional metal materials are prone to corrosion. Polymer-based materials are not suitable for high-band applications, making it difficult to achieve 'thin, light, wide and strong' Features.
The Mg-Ag-Sn-type porous magnesium alloy is prepared by Gasar directional solidification process to control the content and solidification rate of Ag and Sn elements to form a porous magnesium alloy with a composite pore structure, improve conductivity and mechanical properties, and enhance electromagnetic shielding efficiency. .
The balance of high electromagnetic shielding efficiency, lightweight and structural strength is achieved. The conductivity is improved through the Ag element and the Sn element improves the strength, forming an adjustable pore structure, enhancing the energy reduction ability of electromagnetic waves, reducing the material's own weight and simplifying the processing difficulty.
Smart Images

Figure CN118932232A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a porous magnesium alloy with high electromagnetic shielding effectiveness and a preparation method thereof, belonging to the technical application field of porous alloy materials. Background Art
[0002] The rapid development of electronic information technology has brought about serious electromagnetic radiation and interference problems. Excessive use of electronic products leads to electromagnetic pollution, which not only affects communications, but also harms human health and the natural environment. In the military field, taking effective electromagnetic shielding measures to prevent the enemy from destroying electronic equipment is the key to winning modern wars. Ideal electromagnetic shielding materials should have the characteristics of "thin, light, wide and strong", that is, they can achieve strong absorption of electromagnetic waves in a wide frequency band with a small thickness and light weight. Therefore, the development of electromagnetic shielding materials with excellent performance is attracting the attention of various researchers.
[0003] At present, commonly used electromagnetic shielding materials include: metal materials, polymer-based materials and filled composite materials. Traditional metal electromagnetic shielding materials such as Fe, Ni, Cu, Al, etc. have excellent performance, but their high specific gravity and easy corrosion restrict their application. Most polymer-based shielding materials are not suitable for high-band electromagnetic shielding. Electromagnetic shielding materials must have excellent electromagnetic shielding performance and meet the requirements of lightweight, sufficient structural strength, heat dissipation, etc.
[0004] Magnesium alloy is the lightest metal structural material in the world. It has the advantages of low density, good thermal conductivity, good electrical conductivity, high specific strength and specific stiffness, and also has obvious advantages in electromagnetic shielding. The addition of different elements in magnesium-based alloys will affect the performance of magnesium alloys. Ag element can improve the conductivity of the alloy, and the addition of Sn element promotes the formation of Mg2Sn and improves the mechanical properties of the material.
[0005] Gasar directional solidification process is a method for preparing porous metals by using the different solubility of gases in metal liquid / solid phase to cause supersaturated gas precipitation during phase change. In the preparation process of porous alloys, the different types and contents of elements will affect the solidification mode during the alloy solidification process, and the different solidification modes will have an important impact on the pore structure of the final porous alloy.
[0006] Therefore, for porous alloy shielding materials, whether the composition and content within the alloy can be optimized and balanced will be the key to whether the material can meet the current requirements for new electromagnetic shielding materials with high strength, good shielding properties and light weight. Summary of the invention
[0007] The purpose of the present invention is to provide a porous magnesium alloy with high electromagnetic shielding effectiveness, which has the characteristics of adjustable pore structure and small specific gravity, and can reduce electromagnetic wave energy and has high electromagnetic shielding effectiveness.
[0008] In order to solve the above technical problems and achieve corresponding technical effects, the present invention is implemented through the following technical solutions:
[0009] One object of the present invention is to provide a porous magnesium alloy with high electromagnetic shielding effectiveness, the alloy is a Mg-Ag-Sn alloy, containing the following percentages of components: Ag content is 1%-15wt%, Sn content is 0.5%-5wt%, and the rest is Mg;
[0010] Further preferably, the porous magnesium alloy with high electromagnetic shielding effectiveness comprises: Ag content of 4%-6.5wt%, Sn content of 1%-1.5wt%, and the rest of Mg;
[0011] Another object of the present invention is to provide a method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness, comprising the following steps:
[0012] S1: Preparation of magnesium alloy: High-purity Mg, Ag and Sn were used as experimental raw materials. The three elements were mixed and placed in a melting crucible in a reactor. -2 Pa conditions, heated until completely melted and kept warm;
[0013] S2: After S1 is completed, the working gas and the protective gas are introduced into the reaction furnace to a given pressure, and the temperature is kept to obtain a mixed melt;
[0014] S3: After S2 is completed, the mixed melt is solidified by a directional solidification system, and the solidification rate is controlled;
[0015] S4: After the temperature in the reaction furnace in S3 is lowered to room temperature, a porous magnesium alloy with high electromagnetic shielding effectiveness is obtained;
[0016] Furthermore, the purity of Mg, Ag and Sn in the S1 is 99.99%; the heating operation is to slowly increase the temperature first and then quickly increase the temperature to 960° C.; the holding time is 10 minutes;
[0017] Furthermore, in S2, the working gas is high-purity hydrogen with a pressure range of 0-2MPa; the protective gas is high-purity argon with a pressure of 0-2MPa; during ventilation, the superheat of the mixed melt is maintained at 200K; the insulation time is 20min;
[0018] Furthermore, in S3, the cooling and solidification rate is 10-150K / min; the cooling and solidification rate is adjusted by controlling the water flow rate of the water-cooled base in the reaction furnace;
[0019] Furthermore, in S4, when the temperature in the reaction furnace drops to room temperature, the gas in the reaction furnace needs to be discharged by opening the vent valve, the circulating water cooling system needs to be closed, and the furnace cover needs to be opened to take out a porous magnesium alloy with adjustable pore structure and high electromagnetic shielding effectiveness;
[0020] Furthermore, the porous magnesium alloy with high electromagnetic shielding effectiveness has a pore size range of 500 μm-1500 μm, a porosity of 10%-30%, and a through-hole ratio of 20%-65%;
[0021] Compared with the prior art, the present invention provides a porous magnesium alloy with high electromagnetic shielding effectiveness, which mainly has the following beneficial effects:
[0022] 1. The porous magnesium alloy with high electromagnetic shielding effectiveness prepared by the above technical solution has a composite pore structure with coexistence of through pores and closed pores, and the pore structure is adjustable;
[0023] 2. The addition of Ag and Sn elements to magnesium-based metals overcomes the problem of insufficient electrical conductivity and magnetic conductivity of pure magnesium. Specifically: the introduction of Ag elements improves the conductivity of the alloy and thus improves the shielding effectiveness; the addition of Sn elements promotes the formation of Mg2Sn, effectively improving the strength of porous magnesium alloys; at the same time, Ag 17 Mg 54 The appearance of the Mg2Sn phase increases the multiple reflection loss and can improve the shielding performance;
[0024] 3. The composite pore structure with through-holes and closed-holes can not only effectively play the lightweight advantage of the product, but also the pore structure of the through-holes is conducive to air convection, which can effectively and timely guide the energy generated by the operation of electronic equipment to ensure the stable operation of electronic equipment; the pore structure of the closed-holes increases the internal interface of the material, and the reflection loss will increase after the electromagnetic wave is incident, thereby reducing the electromagnetic wave energy and improving the shielding performance;
[0025] 4. Realize the controllable pore size of porous electromagnetic shielding materials. Specifically: by controlling the content of other elements in magnesium-based alloys, especially the content of Ag element (Ag 17 Mg 54 The difference in phase content will cause the porous magnesium alloy to present different solidification modes during the solidification process, from plane to cellular and finally to dendrite, which will effectively regulate the pore structure (pore size, porosity, and through-hole ratio) of the porous magnesium alloy;
[0026] 5. The porous magnesium alloy electromagnetic shielding material prepared by the present invention not only ensures the electromagnetic shielding performance of the material, but also reduces the weight of the shielding material by optimizing the content of Ag and Sn elements and using the directional solidification process. At the same time, the aperture of the porous alloy is simple and easy to adjust, which reduces the difficulty of processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the furnace structure of the Gasar directional solidification device of the present invention; DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] Preparation of Mg-4Ag-Sn porous magnesium alloy electromagnetic shielding material
[0031] (1) Preparation of magnesium alloy;
[0032] (2) Open the gas inlet valve and introduce the working gas H2 and the protective gas Ar into the furnace to a given pressure;
[0033] (3) After the insulation is completed, the melt is poured into the directional solidification system through a graphite funnel, and the solidification rate is adjusted by controlling the water flow rate of the water cooling base;
[0034] (4) When the temperature inside the furnace drops to room temperature, open the vent valve to release the gas in the furnace, open the furnace cover to take out the sample, and finally close the circulating water cooling system.
[0035] In the step (1) of preparing the Mg-Ag-Sn alloy, the Ag content is 4wt%, the Sn content is 1wt%, and the rest is Mg. Mg, Ag and Sn with a purity of 99.99% are used as experimental raw materials; the required elements are placed in a melting crucible, and the furnace is evacuated to 10 -2 Pa; first slowly increase the temperature to make the alloy heated evenly, and quickly increase the temperature to 960℃ to reduce the burning rate, so that all elements in the alloy are completely melted, and keep the temperature for 10 minutes;
[0036] The pressure of the working gas H2 introduced in step (2) is 1 MPa, and the pressure of the protective gas Ar is 0.2 MPa; the superheat of the melt is maintained at 200K during ventilation; the holding time is 20 minutes;
[0037] The cooling and solidification rate in step (3) is 80K / min.
[0038] The coaxial line transmission method is used to test the electromagnetic protection performance. The vector network analyzer is connected to the micro-coaxial shielding effectiveness test device through a cable. The sample is placed in the fixture of the shielding effectiveness test device. Multiple shielding effectiveness tests are carried out and the shielding effectiveness of the material is finally obtained after averaging.
[0039] Example 2
[0040] Preparation of Mg-5Ag-Sn Porous Alloy Electromagnetic Shielding Material
[0041] (1) Preparation of magnesium alloy;
[0042] (2) Open the gas inlet valve and introduce the working gas H2 and the protective gas Ar into the furnace to a given pressure;
[0043] (3) After the insulation is completed, the melt is poured into the directional solidification system through a graphite funnel, and the solidification rate is adjusted by controlling the water flow rate of the water cooling base;
[0044] (4) When the temperature inside the furnace drops to room temperature, open the vent valve to release the gas in the furnace, open the furnace cover to take out the sample, and finally close the circulating water cooling system.
[0045] In the step (1) of preparing the Mg-Ag-Sn alloy, the Ag content is 5wt%, the Sn content is 1wt%, and the rest is Mg. Mg, Ag and Sn with a purity of 99.99% are used as experimental raw materials; the required elements are placed in a melting crucible, and the furnace is evacuated to 10 -2 Pa; first slowly increase the temperature to make the alloy heated evenly, and quickly increase the temperature to 960℃ to reduce the burning rate, so that all elements in the alloy are completely melted, and keep the temperature for 10 minutes;
[0046] The pressure of the working gas H2 introduced in step (2) is 1.5 MPa, and the pressure of the protective gas Ar is 0.5 MPa; the superheat of the melt is maintained at 200K during ventilation; the holding time is 20 minutes;
[0047] The cooling and solidification rate in step (3) is 80K / min.
[0048] The coaxial line transmission method is used to test the electromagnetic protection performance. The vector network analyzer is connected to the micro-coaxial shielding effectiveness test device through a cable. The sample is placed in the fixture of the shielding effectiveness test device. Multiple shielding effectiveness tests are carried out and the shielding effectiveness of the material is finally obtained after averaging.
[0049] Example 3
[0050] Preparation of Mg-6.5Ag-1.5Sn Porous Alloy Electromagnetic Shielding Material
[0051] (1) Preparation of magnesium alloy;
[0052] (2) Open the gas inlet valve and introduce the working gas H2 and the protective gas Ar into the furnace to a given pressure;
[0053] (3) After the insulation is completed, the melt is poured into the directional solidification system through a graphite funnel, and the solidification rate is adjusted by controlling the water flow rate of the water cooling base;
[0054] (4) When the temperature inside the furnace drops to room temperature, open the vent valve to release the gas in the furnace, open the furnace cover to take out the sample, and finally close the circulating water cooling system.
[0055] In the step (1) of preparing the Mg-Ag-Sn alloy, the Ag content is 6.5wt%, the Sn content is 1.5wt%, and the rest is Mg. Mg, Ag and Sn with a purity of 99.99% are used as experimental raw materials; the required elements are placed in a melting crucible, and the furnace is evacuated to 10 -2 Pa; first slowly increase the temperature to make the alloy heated evenly, and quickly increase the temperature to 960℃ to reduce the burning rate, so that all elements in the alloy are completely melted, and keep the temperature for 10 minutes;
[0056] The pressure of the working gas H2 introduced in step (2) is 2 MPa, and the pressure of the protective gas Ar is 0.5 MPa; the superheat of the melt is maintained at 200K during ventilation; the holding time is 20 minutes;
[0057] The cooling and solidification rate in step (3) is 80K / min.
[0058] The coaxial line transmission method is used to test the electromagnetic protection performance. The vector network analyzer is connected to the micro-coaxial shielding effectiveness test device through a cable. The sample is placed in the fixture of the shielding effectiveness test device. Multiple shielding effectiveness tests are carried out and the shielding effectiveness of the material is finally obtained after averaging.
[0059] Table 1 is a statistical table of product performance in Examples 1-3
[0060]
[0061]
[0062] Table 1
[0063] In summary, the porous magnesium alloy with adjustable composite pore structure and high electromagnetic shielding efficiency prepared by the present invention: by optimizing the content of each element Ag and Sn and using the directional solidification process, it not only ensures the electromagnetic shielding performance of the material, but also reduces the self-weight of the shielding material; the composite pore structure of through holes and closed holes optimizes the thermal conductivity of the material on the one hand, and increases the reflection loss of the incident electromagnetic wave on the other hand, thereby improving the overall performance of the shielding material; the overall structural dimensions (pore size, porosity, and through hole ratio) of the shielding material are stable and controllable, simple to process, and can effectively adapt to different working conditions.
[0064] Example 4
[0065] In this embodiment, a preparation device for a porous magnesium alloy with high electromagnetic shielding effectiveness is introduced. The device is used for the specific implementation of the preparation method described in the technical solution of the present invention, and is used for the preparation of the porous magnesium alloy with high shielding effectiveness in the above embodiments 1-3. Specifically, a preparation device for a porous magnesium alloy with high electromagnetic shielding effectiveness:
[0066] The preparation device comprises: a vacuum system, a circulating water cooling system, a smelting system, a gas charging and discharging system and a directional solidification system; the vacuum system is a reaction furnace with a closed space;
[0067] A top cover is installed on the top of the reactor, and an air inlet valve and an air outlet valve are installed on the top cover respectively, and an observation window is opened; the upper space in the reactor is a smelting system, and the lower space is a directional solidification system;
[0068] The smelting system is provided with a smelting crucible, and an induction coil is provided on the outer wall of the smelting crucible; the smelting system is connected to the directional solidification system through a funnel with upper and lower ends opened, and the mixed melt in the smelting crucible enters the directional solidification system through the funnel;
[0069] The directional solidification system comprises: a solidification crucible and a circulating water cooling system; the solidification crucible is located below the funnel, the circulating water cooling system comprises a quenching copper seat and a water storage tank, the water storage tank is provided with a water inlet and a water outlet respectively, and water is introduced into the water inlet and discharged from the water outlet to realize water circulation; the quenching copper seat is located on the water storage tank and below the solidification crucible;
[0070] The top cover and the furnace body of the reaction furnace are locked by a locking device;
[0071] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A porous magnesium alloy with high electromagnetic shielding effectiveness, characterized in that: The porous magnesium alloy with high electromagnetic shielding effectiveness is a Mg-Ag-Sn alloy, which contains the following components in percentages: Ag content is 1%-15wt%, Sn content is 0.5%-5wt%, and the rest is Mg.
2. The porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 1, characterized in that: The group contains raw materials with the following component percentages: Ag content is 4%-6.5wt%, Sn content is 1%-1.5wt%, and the rest is Mg.
3. A method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness, characterized in that: The method for preparing a porous magnesium alloy having high electromagnetic shielding effectiveness as claimed in claim 1 comprises the following steps: S1: Preparation of magnesium alloy: High-purity Mg, Ag and Sn were used as experimental raw materials. The three experimental raw materials were mixed and heated for 10 - 2 Pa conditions, heated until completely melted and kept warm; S2: After S1 is completed, the temperature is kept under a given pressure of working gas and protective gas to obtain a mixed melt; S3: After S2 is completed, the mixed melt is solidified by a directional solidification system, and the solidification rate is controlled; S4: After the reaction temperature in S3 is lowered to room temperature, a porous magnesium alloy with high electromagnetic shielding performance is obtained.
4. The method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 3, characterized in that: The purity of Mg, Ag and Sn in the S1 is 99.99%; the heating operation is to slowly increase the temperature first and then quickly increase the temperature to 960° C.; the heat preservation time is 10 minutes.
5. The method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 3, characterized in that: In S2, the working gas is high-purity hydrogen with a pressure range of 0-2MPa; the protective gas is high-purity argon with a pressure of 0-2MPa; during ventilation, the superheat of the mixed melt is maintained at 200K; and the insulation time is 20min.
6. The method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 3, characterized in that: In S3, the cooling and solidification rate ranges from 10 to 150 K / min; the cooling and solidification rate is adjusted by controlling the water flow rate.
7. The method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 3, characterized in that: In S4, after the reaction temperature is lowered to room temperature, the reaction gas is removed and the circulating water cooling system is closed to obtain a porous magnesium alloy with adjustable pore structure and high electromagnetic shielding performance.
8. The method for preparing a porous magnesium alloy with high electromagnetic shielding effectiveness according to claim 3, characterized in that: The porous magnesium alloy with high electromagnetic shielding effectiveness has a pore size range of 500 μm-1500 μm, a porosity of 10%-30%, and a through-hole ratio of 20%-65%.
Citation Information
Cited By
Bright rod preparation device with four-layer structure crystallizer and method
CN121267123A