Alkali-activated fly ash colloid grouting integrated device, grouting method, alkali-activated fly ash colloid and preparation method of alkali-activated fly ash colloid
Through the integrated grouting device for alkali-activated fly ash colloids, the problem of easy pipe blockage and poor fluidity of fly ash grouting materials is solved, forming high-flow and stable alkali-activated fly ash colloids, realizing the sustainable resource Utilization and environmental protection requirements simplify the process flow and improve production efficiency.
Patent Information
- Application Number
- CN202410994714.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing fly ash grouting materials are prone to pipe blockage, poor fluidity, and high energy consumption, which affect their application effect and economy.
The integrated grouting device for colloidal grouting of alkali-excited fly ash is used to achieve accurate mixing and grouting of fly ash through automatic proportioning and pneumatic pump device, and the Si, Al and Ca elements in fly ash are stimulated by alkali-excited agents. Form a gel with a three-dimensional network structure to improve fluidity and stability.
It improves the flowability and stability of fly ash colloids, reduces production costs, realizes sustainable utilization of resources and environmental protection requirements, simplifies process flow, and improves production efficiency.
Smart Images

Figure CN118934009A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fly ash colloid, and in particular to an alkali-activated fly ash colloid grouting integrated device and grouting method, alkali-activated fly ash colloid and a preparation method thereof. Background Art
[0002] Fly ash is a fine particle produced when burning coal. It is mainly composed of inorganic substances such as silicon oxide and aluminum oxide and is often treated as industrial waste. However, in recent years, with the advancement of mining technology and the emphasis on resource utilization, the recycling of fly ash as a resource has received widespread attention. Traditional treatment methods mainly rely on landfill or simple stacking, which results in resource waste and environmental pollution. At the same time, mining environmental safety has also received much attention. Abandoned fly ash may pose a potential threat to soil, water sources and ecosystems.
[0003] At present, fly ash slurry is commonly used as a filling material for filling abandoned space in mines, which can effectively utilize abandoned space in mines, reduce resource waste, and reduce the risk of surface subsidence and geological disasters in mines. However, the existing fly ash slurry may encounter challenges such as pipe blockage, poor fluidity, insufficient adhesion, high cost, environmental problems and insufficient stability during application, which affect the actual application effect and economy of fly ash slurry. Summary of the invention
[0004] The purpose of the present invention is to provide an alkali-activated fly ash colloid grouting integrated device and grouting method, alkali-activated fly ash colloid and its preparation method, so as to solve the problems of existing fly ash grouting materials such as easy pipe clogging, poor fluidity and high energy consumption.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an alkali-activated fly ash colloid grouting integrated device, comprising an automatic proportioning device 1, a mixing device 2, and a pneumatic pump device 3 connected in sequence;
[0007] The automatic proportioning device 1 includes a dry material proportioning unit, a water material proportioning unit, a pressure sensor 1-5, a flow sensor 1-6 and an automatic proportioning system 1-9;
[0008] The dry material proportioning unit includes a dry material inlet 1-1, a dry material agitator 1-3 and a material quality controller 1-7; the water material proportioning unit includes a water inlet 1-2, a water agitator 1-4 and a water material quality controller 1-8;
[0009] The dry material inlet 1-1, the dry material agitator 1-3 and the material quality controller 1-7 are connected in sequence;
[0010] The water inlet 1-2, the water agitator 1-4 and the water material quality controller 1-8 are connected in sequence;
[0011] The mixing device 2 comprises a stirring tank 2-1;
[0012] The dry material inlet 1-1 is connected to the mixing tank 2-1; the pressure sensor 1-5 and the flow sensor 1-6 are arranged on the connecting pipe between the dry material inlet 1-1 and the mixing tank 2-1;
[0013] The water inlet 1-2 is connected to the mixing tank 2-1; the pressure sensor 1-5 and the flow sensor 1-6 are arranged on the connecting pipe between the water inlet 1-2 and the mixing tank 2-1;
[0014] The pneumatic pump device 3 includes a pneumatic diaphragm pump 3-1, an air supply port 3-2, an automatic regulating valve 3-3, a display device 3-4, a first pump chamber connecting shaft 3-5, a piston 3-6, a first pump chamber 3-7, a first pump chamber diaphragm 3-9, a first pump chamber drive chamber 3-10, a second pump chamber drive chamber 3-11, a second pump chamber diaphragm 3-12, a second pump chamber 3-13, a compressed air device 3-17 and a delivery pipeline 3-18;
[0015] The stirring tank 2-1 is connected to the delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1;
[0016] The pneumatic diaphragm pump 3-1 is provided with a first pump chamber 3-7 and a second pump chamber 3-13, the first pump chamber 3-7 and the second pump chamber 3-13 are connected by a first pump chamber connecting shaft 3-5, a piston 3-6 is provided on the first chamber connecting shaft 3-5, and a first pump chamber driving chamber 3-10 and a second pump chamber driving chamber 3-11 are provided on the first pump chamber 3-7 and the second pump chamber 3-13, respectively; a first pump chamber diaphragm 3-9 and a second pump chamber diaphragm 3-10 and a second pump chamber diaphragm 3-11 are provided in the first pump chamber driving chamber 3-10 and the second pump chamber driving chamber 3-11, respectively. The first pump chamber drive chamber 3-10 and the second pump chamber drive chamber 3-11 are respectively connected to the air supply port 3-2 on the outside of the pneumatic diaphragm pump 3-1, and the automatic regulating valve 3-3 and the display device 3-4 are arranged on the connecting pipe between the first pump chamber drive chamber 3-10, the second pump chamber drive chamber 3-11 and the air supply port 3-2; the air supply port 3-2 is connected to the compressed air device 3-17 through the first pipe 3-16; the first pump chamber 3-7 and the second pump chamber 3-13 are also connected through the delivery pipe 3-18.
[0017] Preferably, in the above-mentioned alkali-activated fly ash colloid grouting integrated device, the mixing device 2 further includes an electric stirrer 2-2, a stirring blade 2-3, a ball valve 2-4 and a flow meter 2-5;
[0018] An electric stirrer 2-2 is arranged outside the stirring tank 2-1, and a stirring blade 2-3 is arranged at the bottom of the stirring tank 2-1, and the stirring blade 2-3 is connected to the electric stirrer 2-2;
[0019] The ball valve 2-4 and the flow meter 2-5 are arranged on the connecting pipe between the stirring tank 2-1 and the delivery pipe 3-18 in the pneumatic diaphragm pump 3-1.
[0020] Preferably, in the above-mentioned alkali-activated fly ash colloid grouting integrated device, the pneumatic pump device 3 further includes a one-way valve 3-8;
[0021] The delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1 is connected to the goaf 4 through a discharge pipeline;
[0022] The one-way valve 3-8 is arranged on the delivery pipe 3-18 connecting the first pump chamber 3-7 and the second pump chamber 3-13;
[0023] The pressure sensor 3-14 and the flow sensor 3-15 are arranged on the discharge pipe connecting the delivery pipe 3-18 in the pneumatic diaphragm pump 3-1 and the goaf 4.
[0024] The present invention also provides a method for integrated grouting using the above-mentioned alkali-activated fly ash colloid grouting integrated device, comprising the following steps:
[0025] Add dry material into the dry material proportioning unit, add water material into the water material proportioning unit, mix the dry material and the water material in the stirring tank 2-1 to obtain alkali-activated fly ash colloid, and grout the obtained alkali-activated fly ash colloid into the goaf 4 through the pneumatic pump device 3.
[0026] The present invention also provides an alkali-activated fly ash colloid prepared by the above-mentioned alkali-activated fly ash colloid grouting integrated device, which is prepared from the following raw materials in parts by weight:
[0027] 0.1-0.5 parts of anionic polysaccharide macromolecular substance, 0.1-0.5 parts of macromolecular polymer, 10-30 parts of fly ash, 1-5 parts of alkali activator, 20-60 parts of water;
[0028] The anionic polysaccharide macromolecular substance is xanthan gum or guar gum;
[0029] The high molecular polymer is carbomer or welan gum.
[0030] Preferably, in the above-mentioned alkali-activated fly ash colloid, the alkali activator is sodium hydroxide.
[0031] Preferably, in the above-mentioned alkali-activated fly ash colloid, the particle size of the fly ash is 0.01 to 200 μm.
[0032] The present invention also provides a method for preparing alkali-activated fly ash colloid, comprising the following steps:
[0033] The alkali activator, fly ash and water are first mixed to obtain alkali activated fly ash filtrate and alkali activated fly ash through separation;
[0034] The alkali-activated fly ash filtrate is added to the water-material proportioning unit, the alkali-activated fly ash, anionic polysaccharide macromolecular substance and macromolecular polymer are added to the dry material proportioning unit, the fly ash filtrate and the mixture of alkali-activated fly ash, anionic polysaccharide macromolecular substance and macromolecular polymer are mixed in the stirring tank 2-1 to obtain alkali-activated fly ash colloid.
[0035] Preferably, in the above-mentioned method for preparing alkali-activated fly ash colloid, the temperature of the first mixing is 40 to 70° C., and the time of the first mixing is 12 to 48 hours.
[0036] The mechanism of alkali-activated fly ash colloid in the present invention is: under the chemical action of a strong activator, mainly OH - Ions corrode fly ash, causing Si, Al, Ca and other elements in fly ash to enter the activator solution in the form of ions, reacting chemically with the sodium hydroxide in the solution, causing the Si-O-Si, Al-O-Al and Si-O-Al bonds to break, causing the [SiO4] or [AlO4] tetrahedral network structure in fly ash to depolymerize, forming Al(OH)4 or 3Al(OH)6, Si(OH)3 or SiO2(OH) or SiO3(OH)3 and other complexes. - Under catalysis, the silicon-aluminum monomers rearrange to form silicate and aluminate oligomeric complexes. The high activity of Al(OH)4 makes aluminate and silicate complexes easier to condense. Sol particles bind to Na by coordination bonds or electrostatic bonds. + Further condensation forms gel particles, forming a three-dimensional network structure, and finally forming a reaction product (CSH / CASH / NASH gel). This gel plays a role in improving fluidity, gelling, enhancing stability and filling in alkali-activated fly ash colloid.
[0037] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The present invention adopts a pneumatic pump and an automatic proportioning device to realize the automation of the process, the integration of the pneumatic pump and the optimization of the process parameters. The automatic proportioning part includes a sensor and a monitoring equipment quality controller. By real-time monitoring of key parameters and cooperating with a computer control system (automatic proportioning system), the accurate proportioning of fly ash colloid raw materials is realized and the stability of the proportioning is ensured. The pneumatic pump device part adopts a pneumatic diaphragm pump to realize the suction and discharge of the mining fly ash colloid, introduces process parameter optimization, and optimizes the process parameters through experiments and data analysis to obtain the best grouting effect. Automatic control ensures comprehensive control of the system and optimization of the grouting process. The integrated mining fly ash colloid grouting process can share data and coordinate with each other, simplify the process flow, and improve production efficiency and proportioning accuracy. Through process optimization and precise control, the effect of energy saving and emission reduction is achieved, environmental protection requirements are met, and production costs are reduced.
[0039] (2) Compared with traditional fly ash grouting materials, the alkali-activated fly ash colloid prepared by the present invention has stronger water retention, stability and fluidity. After the fly ash is activated, the glass structure is destroyed, and the soluble SiO2 and Al2O3 rich in the glass react chemically with Ca(OH)2 to generate a gel system composed of a three-dimensional network structure of aluminum silicate polymers composed of [AlO4] and [SiO4] tetrahedral structural units and aluminum-containing hydrated calcium silicate gel, which further improves the fluidity and stability of the fly ash colloid.
[0040] (3) The present invention uses solid waste fly ash as aggregate, processes it with the aid of alkali activation technology, fully utilizes the active components of fly ash, and realizes sustainable utilization of resources. A mining alkali-activated fly ash colloid with good fluidity, strong water retention, and green environmental protection is prepared by physical blending. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.
[0042] Figure 1It is an integrated alkali-activated fly ash colloid grouting device of the present invention; wherein 1 is an automatic proportioning device, 2 is a mixing device, 3 is a pneumatic pump device, and 4 is a goaf; 1-1 is a dry material inlet, 1-2 is a water inlet, 1-3 is a dry material agitator, 1-4 is a water agitator, 1-5 is a pressure sensor, 1-6 is a flow sensor, 1-7 is a material quality controller, 1-8 is a water material quality controller, 1-9 is an automatic proportioning system, 2-1 is a stirring tank, 2-2 is an electric stirrer, 2-3 is a stirring blade, 2-4 is a ball valve, and 2-5 is a flow meter , 3-1 is a pneumatic diaphragm pump, 3-2 is an air supply port, 3-3 is an automatic regulating valve, 3-4 is a display device, 3-5 is a first pump chamber connecting shaft, 3-6 is a piston, 3-7 is a first pump chamber, 3-8 is a one-way valve, 3-9 is a first pump chamber diaphragm, 3-10 is a first pump chamber drive chamber, 3-11 is a second pump chamber drive chamber, 3-12 is a second pump chamber diaphragm, 3-13 is a second pump chamber, 3-14 is a pressure sensor, 3-15 is a flow sensor, 3-16 is a first pipeline, 3-17 is a compressed air device, and 3-18 is a delivery pipeline;
[0043] Figure 2 The present invention is a flow chart for preparing the alkali-activated fly ash colloid;
[0044] Figure 3 This is a sample diagram of the alkali-activated fly ash colloid in Example 7;
[0045] Figure 4 The scanning electron microscope image and element distribution map of the fly ash in Example 3; wherein (a) is a scanning electron microscope image of the fly ash with a scale of 10 μm, (b) is a scanning electron microscope image of the fly ash with a scale of 1 μm, and (c) is an element distribution map of the fly ash;
[0046] Figure 5 The scanning electron microscope images and element distribution diagrams of the alkali-activated fly ash in Example 3; (a) is a scanning electron microscope image of the alkali-activated fly ash with a scale of 10 μm, (b) is a scanning electron microscope image of the alkali-activated fly ash with a scale of 1 μm, and (c) is an element distribution diagram of the alkali-activated fly ash;
[0047] Figure 6 This is the particle size distribution diagram of the alkali-activated fly ash and fly ash in Example 3. DETAILED DESCRIPTION
[0048] The present invention provides an alkali-activated fly ash colloid grouting integrated device, comprising an automatic proportioning device 1, a mixing device 2, and a pneumatic pump device 3 connected in sequence;
[0049] The automatic proportioning device 1 includes a dry material proportioning unit, a water material proportioning unit, a pressure sensor 1-5, a flow sensor 1-6 and an automatic proportioning system 1-9;
[0050] The dry material proportioning unit includes a dry material inlet 1-1, a dry material agitator 1-3 and a material quality controller 1-7; the water material proportioning unit includes a water inlet 1-2, a water agitator 1-4 and a water material quality controller 1-8;
[0051] The dry material inlet 1-1, the dry material agitator 1-3 and the material quality controller 1-7 are connected in sequence;
[0052] The water inlet 1-2, the water agitator 1-4 and the water material quality controller 1-8 are connected in sequence;
[0053] The mixing device 2 comprises a stirring tank 2-1;
[0054] The dry material inlet 1-1 is connected to the mixing tank 2-1; the pressure sensor 1-5 and the flow sensor 1-6 are arranged on the connecting pipe between the dry material inlet 1-1 and the mixing tank 2-1;
[0055] The water inlet 1-2 is connected to the mixing tank 2-1; the pressure sensor 1-5 and the flow sensor 1-6 are arranged on the connecting pipe between the water inlet 1-2 and the mixing tank 2-1;
[0056] The pneumatic pump device 3 includes a pneumatic diaphragm pump 3-1, an air supply port 3-2, an automatic regulating valve 3-3, a display device 3-4, a first pump chamber connecting shaft 3-5, a piston 3-6, a first pump chamber 3-7, a first pump chamber diaphragm 3-9, a first pump chamber drive chamber 3-10, a second pump chamber drive chamber 3-11, a second pump chamber diaphragm 3-12, a second pump chamber 3-13, a compressed air device 3-17 and a delivery pipeline 3-18;
[0057] The stirring tank 2-1 is connected to the delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1;
[0058] The pneumatic diaphragm pump 3-1 is provided with a first pump chamber 3-7 and a second pump chamber 3-13, the first pump chamber 3-7 and the second pump chamber 3-13 are connected by a first pump chamber connecting shaft 3-5, a piston 3-6 is provided on the first chamber connecting shaft 3-5, and a first pump chamber driving chamber 3-10 and a second pump chamber driving chamber 3-11 are provided on the first pump chamber 3-7 and the second pump chamber 3-13, respectively; a first pump chamber diaphragm 3-9 and a second pump chamber diaphragm 3-10 and a second pump chamber diaphragm 3-11 are provided in the first pump chamber driving chamber 3-10 and the second pump chamber driving chamber 3-11, respectively. The first pump chamber drive chamber 3-10 and the second pump chamber drive chamber 3-11 are respectively connected to the air supply port 3-2 on the outside of the pneumatic diaphragm pump 3-1, and the automatic regulating valve 3-3 and the display device 3-4 are arranged on the connecting pipe between the first pump chamber drive chamber 3-10, the second pump chamber drive chamber 3-11 and the air supply port 3-2; the air supply port 3-2 is connected to the compressed air device 3-17 through the first pipe 3-16; the first pump chamber 3-7 and the second pump chamber 3-13 are also connected through the delivery pipe 3-18.
[0059] In the present invention, the mixing device 2 further includes an electric stirrer 2-2, a stirring blade 2-3, a ball valve 2-4 and a flow meter 2-5;
[0060] An electric stirrer 2-2 is arranged outside the stirring tank 2-1, and a stirring blade 2-3 is arranged at the bottom of the stirring tank 2-1, and the stirring blade 2-3 is connected to the electric stirrer 2-2;
[0061] The ball valve 2-4 and the flow meter 2-5 are arranged on the connecting pipe between the stirring tank 2-1 and the delivery pipe 3-18 in the pneumatic diaphragm pump 3-1.
[0062] In the present invention, the pneumatic pump device 3 further includes a one-way valve 3-8;
[0063] The delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1 is connected to the goaf 4 through a discharge pipeline;
[0064] The one-way valve 3-8 is arranged on the delivery pipe 3-18 connecting the first pump chamber 3-7 and the second pump chamber 3-13;
[0065] The pressure sensor 3-14 and the flow sensor 3-15 are arranged on the discharge pipe connecting the delivery pipe 3-18 in the pneumatic diaphragm pump 3-1 and the goaf 4.
[0066] The present invention also provides a method for integrated grouting using the above-mentioned alkali-activated fly ash colloid grouting integrated device, comprising the following steps:
[0067] Add dry material into the dry material proportioning unit, add water material into the water material proportioning unit, mix the dry material and the water material in the stirring tank 2-1 to obtain alkali-activated fly ash colloid, and grout the obtained alkali-activated fly ash colloid into the goaf 4 through the pneumatic pump device 3.
[0068] The present invention also provides an alkali-activated fly ash colloid prepared by the above-mentioned alkali-activated fly ash colloid grouting integrated device, which is prepared from the following raw materials in parts by weight:
[0069] 0.1-0.5 parts of anionic polysaccharide macromolecular substance, 0.1-0.5 parts of macromolecular polymer, 10-30 parts of fly ash, 1-5 parts of alkali activator, and 20-60 parts of water.
[0070] In the present invention, the mass fraction of the anionic polysaccharide polymer substance is preferably 0.1 to 0.5 parts, more preferably 0.2 to 0.4 parts, and even more preferably 0.3 parts.
[0071] In the present invention, the mass fraction of the high molecular weight polymer is preferably 0.1 to 0.5 parts, more preferably 0.2 to 0.4 parts, and even more preferably 0.3 parts.
[0072] In the present invention, the mass fraction of the fly ash is preferably 10 to 30 parts, more preferably 15 to 25 parts, and even more preferably 18 to 22 parts.
[0073] In the present invention, the mass fraction of the base activator is preferably 1 to 5 parts, more preferably 2 to 4 parts, and more preferably 3 parts.
[0074] In the present invention, the mass fraction of the water is preferably 20 to 60 parts, more preferably 25 to 55 parts, and even more preferably 30 to 40 parts.
[0075] In the present invention, the anionic polysaccharide polymer is preferably xanthan gum or guar gum, more preferably xanthan gum. Xanthan gum is composed of D-glucose, D-mannose and D-glucuronic acid, generally made into sodium, potassium or calcium salt, has strong hydration ability and dispersion stability, and can form a stable three-dimensional network structure in aqueous solution. This network structure can coat and stabilize fly ash particles, prevent them from settling and aggregating, and maintain the uniform dispersion state of the colloid.
[0076] In the present invention, the high molecular polymer is preferably carbomer or welan gum, and more preferably carbomer. Carbomer is a polymer formed by chemical cross-linking of acrylic acid or acrylic acid ester and allyl ether, and its carboxyl group is ionized. Due to the mutual repulsion of negative charges, the curled molecular chain stretches to a great expansion state, increasing the original volume to about 1000 times, thereby playing a thickening role.
[0077] In the present invention, the alkaline activator is preferably sodium hydroxide.
[0078] In the present invention, the fly ash is preferably Class I F fly ash.
[0079] In the present invention, the particle size of the fly ash is preferably 0.01-200 μm, the fly ash with a particle size less than 12.86 μm accounts for 50% of the total mass of the fly ash, and the fly ash with a particle size less than 45.47 μm accounts for 90% of the total mass of the fly ash.
[0080] The present invention also provides a method for preparing alkali-activated fly ash colloid, comprising the following steps:
[0081] The alkali activator, fly ash and water are first mixed to obtain alkali activated fly ash filtrate and alkali activated fly ash through separation;
[0082] The alkali-activated fly ash filtrate is added to the water-material proportioning unit, the alkali-activated fly ash, anionic polysaccharide macromolecular substance and macromolecular polymer are added to the dry material proportioning unit, the fly ash filtrate and the mixture of alkali-activated fly ash, anionic polysaccharide macromolecular substance and macromolecular polymer are mixed in the stirring tank 2-1 to obtain alkali-activated fly ash colloid.
[0083] In the present invention, the addition amount of alkali-activated fly ash is monitored in real time by the material quality controller 1-7, and the addition amount of alkali-activated fly ash is transmitted to the automatic proportioning system 1-9 for processing by the flow sensor 1-6 and the pressure sensor 1-5. The automatic proportioning system 1-9 adjusts the input amount of alkali-activated fly ash, anionic polysaccharide polymer material, and high molecular polymer ingredients through the flow sensor 1-6 according to the preset proportioning ratio and algorithm to achieve accurate proportioning requirements; the water material quality controller 1-8 can accurately control the addition amount of alkali-activated fly ash filtrate to maintain the proportioning accuracy, the pressure sensor 1-5 can monitor the pipeline pressure to ensure system safety and optimize fluid transportation, the flow sensor 1-6 can measure the water material flow rate and accurately control the water material addition amount; at the same time, the pressure sensor 1-5 can work in coordination with the quality controller to monitor the pressure changes and adjust the flow rate to ensure the stability and accuracy of the flow rate.
[0084] In the present invention, the specific process of mixing in the stirring tank 2-1 is:
[0085] The alkali-activated fly ash filtrate and the mixture of alkali-activated fly ash, anionic polysaccharide macromolecular substances and macromolecular polymers are mixed by a stirring blade 2-3 connected to an electric stirrer 2-2 outside the stirring tank to obtain alkali-activated fly ash colloid, wherein the electric stirrer 2-2 provides power to drive the stirring blade 2-3 to rotate so that the materials are mixed evenly, and the ball valve 2-4 and the flowmeter 2-5 are arranged on the connecting pipe between the stirring tank 2-1 and the conveying pipe 3-18 in the pneumatic diaphragm pump 3-1 to adjust the flow rate of the alkali-activated fly ash colloid.
[0086] In the present invention, the automatic regulating valve 3-3 in the pneumatic pump device 3 is used to adjust the air supply, and the display device 3-4 is used to display the opening of the regulating valve. The operation rate is adjusted by adjusting the automatic regulating valve 3-3; the compressed air system 3-17 in the pneumatic pump device 3 compresses the air to the required pressure, and provides stable compressed air for the pneumatic diaphragm pump 3-1. When the pneumatic force acts on the piston 3-16, the first pump chamber 3-7 and the second pump chamber 3-13 compress the gas through the reciprocating motion of the piston 3-6 to form a negative pressure in the conveying pipeline, so that the alkali-activated fly ash colloid generates flow potential energy in the conveying pipeline 3-18, thereby driving the liquid or slurry to be pumped through the pipeline. The pipeline connects the mixing device 2 and the pneumatic pump device 3, and the mixed alkali-activated fly ash colloid is conveyed to the conveying pipeline 3-18 in the pneumatic diaphragm pump 3-1. The ball valve 2-4 is used to control the flow of the alkali-activated fly ash colloid for mining, including starting, stopping and adjusting the flow rate.
[0087] In the present invention, the alkali-activated fly ash colloid is transported to the goaf 4 through the pneumatic pump device 3. The hydraulic and flow working parameters generated by the pneumatic diaphragm pump 3-1 during operation can be used as feedback signals. The feed speed is adjusted according to the flow signal to ensure that the feed amount is appropriate. The hydraulic signal adjusts the pump speed to ensure that the pump is in good working condition. These working parameter signals are input into the automatic proportioning system 1-9 through the pressure sensor 3-14 and the flow sensor 3-15. The control system will adjust and control the automatic proportioning device 1 in real time according to the feedback working parameters to ensure the accuracy and stability of the proportioning to maintain the required proportioning accuracy. Through network connection and data transmission technology, the data of the pneumatic diaphragm pump 3 and the automatic proportioning device 1 are shared into a central monitoring system (automatic proportioning system 1-9), so as to realize real-time monitoring and control of the working status of the two devices, and can be remotely adjusted and optimized.
[0088] In the present invention, the temperature of the first mixing is preferably 40 to 70° C., more preferably 45 to 75° C., and more preferably 50 to 60° C.; the time of the first mixing is preferably 12 to 48 h, more preferably 15 to 30 h, and more preferably 20 to 25 h.
[0089] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0090] The materials used in the examples are as follows:
[0091] The fly ash is preferably Class I F fly ash.
[0092] The particle size of the fly ash is 0.01-200 μm, the fly ash with a particle size less than 12.86 μm accounts for 50% of the total mass of the fly ash, and the fly ash with a particle size less than 45.47 μm accounts for 90% of the total mass of the fly ash.
[0093] Example 1
[0094] 50 parts of fly ash were added to 200 parts of water, and then stirred and mixed in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which was filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate was tested for metal ions using an ICP tester, and the test results showed that Si in the alkali-activated fly ash filtrate was 46.87 mol / L and Al was 42.79 mol / L.
[0095] Example 2
[0096] 2 parts of sodium hydroxide and 50 parts of fly ash were mixed and added to 200 parts of water, and then stirred and mixed in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which was filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate was tested for metal ions using an ICP tester, and the test results showed that Si in the alkali-activated fly ash filtrate was 13666.65 mol / L and Al was 1076.29 mol / L.
[0097] Example 3
[0098] 3 parts of sodium hydroxide and 50 parts of fly ash were mixed and added to 200 parts of water, and then stirred and mixed in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which was filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate was tested for metal ions using an ICP tester, and the test results showed that Si in the alkali-activated fly ash filtrate was 26729.91 mol / L and Al was 2623.26 mol / L.
[0099] The chemical components in the fly ash and the alkali-activated fly ash prepared in Example 3 were detected by X-ray fluorescence spectrometer (XRF). The detection results are shown in Table 1.
[0100] Table 1 Chemical compositions of fly ash and alkali-activated fly ash prepared in Example 3
[0101]
[0102] The scanning electron microscope images and particle size distribution diagrams of the fly ash and alkali-activated fly ash in Example 3 are as follows: Figure 4 , 5 As shown. Figure 4 , 5 It can be seen that after the fly ash is treated with alkali, it can be clearly seen that the hollow spheres are filled with sediments, which appear as needle-shaped and granular gels.
[0103] The particle size distribution diagram of fly ash and alkali activated fly ash in Example 3 is as follows: Figure 6 As shown. Figure 6 It can be seen that the particle size distribution curve of alkali-activated fly ash moves to the left as a whole, and the D 50 and D 90 Both decreased, indicating that the average particle size and the larger particle size decreased.
[0104] Example 4
[0105] 4 parts of sodium hydroxide and 50 parts of fly ash were mixed and added to 200 parts of water, and then stirred and mixed in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which was filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate was tested for metal ions using an ICP tester, and the test results showed that Si in the alkali-activated fly ash filtrate was 23307.28 mol / L and Al was 3936.66 mol / L.
[0106] Example 5
[0107] 5 parts of sodium hydroxide and 50 parts of fly ash were mixed and added to 200 parts of water, and then stirred and mixed in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which was filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate was tested for metal ions using an ICP tester, and the test results showed that Si in the alkali-activated fly ash filtrate was 22632.58 mol / L and Al was 5256.35 mol / L.
[0108] By comparing the test results in Examples 1 to 5, it can be seen that the alkali activation effect in Example 3 is better. When the alkali activator is 3 parts, the Si ion leaching amount of the fly ash filtrate is larger.
[0109] Example 6
[0110] 20 parts of the alkali-activated fly ash prepared in Example 3, 0.25 parts of xanthan gum, and 0.2 parts of carbomer are added to the dry material inlet 1-1 in the dry material proportioning unit, and stirred with the dry material stirrer 1-3 to obtain dry material; the alkali-activated fly ash filtrate prepared in Example 5 is added to the water inlet 1-2 in the water material proportioning unit, and stirred with the water stirrer 1-4 to obtain water material; the addition amount of the alkali-activated fly ash is monitored in real time by the material quality controller 1-7, and the addition amount of the alkali-activated fly ash is transmitted to the automatic proportioning system 1-9 for processing through the flow sensor 1-6 and the pressure sensor 1-5, and the automatic proportioning system 1 -9 According to the preset proportion and algorithm, the input amount of alkali-activated fly ash, xanthan gum and carbomer ingredients is adjusted through flow sensor 1-6 to achieve accurate proportion requirements; the water material quality controller 1-8 can accurately control the amount of alkali-activated fly ash filtrate added to maintain the proportion accuracy, the pressure sensor 1-5 can monitor the pipeline pressure, ensure system safety, optimize fluid transportation, and the flow sensor 1-6 can measure the water material flow rate and accurately control the amount of water material added; at the same time, the pressure sensor 1-5 can work in conjunction with the quality controller to monitor pressure changes and adjust the flow rate to ensure the stability and accuracy of the flow rate;
[0111] The dry material and the water material are stirred in the mixing tank 2-1 by the stirring blade 2-3 connected to the electric mixer 2-2 outside the mixing tank to obtain the alkali-activated fly ash colloid, and the obtained fly ash colloid is pumped into the goaf 4 through the pneumatic pump device 3; wherein the electric mixer 2-2 provides power to drive the stirring blade 2-3 to rotate so that the materials are mixed evenly, and the ball valve 2-4 and the flow meter 2-5 are arranged on the connecting pipe between the mixing tank 2-1 and the conveying pipe 3-18 in the pneumatic diaphragm pump 3-1 to adjust the flow rate of the alkali-activated fly ash colloid;
[0112] The pneumatic pump device 3 includes a pneumatic diaphragm pump 3-1 and a compressed air system 3-17. The air outlet of the compressed air system is connected to the air supply port 3-2 of the pneumatic diaphragm pump 3-1 through a first pipe 3-16. A first pump chamber 3-7 and a second pump chamber 3-13 are arranged in the pneumatic diaphragm pump 3-1. The first pump chamber 3-7 and the second pump chamber 3-13 are connected through a first pump chamber connecting shaft 3-5. A piston 3-6 is arranged on the first chamber connecting shaft 3-5. The first pump chamber 3-7 and the second pump chamber 3-13 are also connected through a conveying pipe 3-18. A first pump chamber drive chamber 3-10 and a second pump chamber drive chamber 3-11 are respectively arranged in the first pump chamber 3-7 and the second pump chamber 3-13; a first pump chamber diaphragm 3-9 and a second pump chamber diaphragm 3-12 are respectively arranged in the first pump chamber drive chamber 3-10 and the second pump chamber drive chamber 3-11. The pump chamber drive chamber 3-11 is respectively connected to the air supply port 3-2 on the outside of the pneumatic diaphragm pump 3-1. An automatic regulating valve 3-3 and a display device 3-4 are respectively arranged on the connecting pipes between the first pump chamber drive chamber 3-10, the second pump chamber drive chamber 3-11 and the air supply port 3-2. The automatic regulating valve 3-3 is used to adjust the air supply volume, and the display device 3-4 is used to display the opening of the regulating valve. The operation rate is adjusted by adjusting the automatic regulating valve 3-3; the compressed air system 3-17 compresses the air to the required pressure and provides stable compressed air for the pneumatic diaphragm pump 3-1. When the pneumatic force acts on the piston 3-6, the first pump chamber 3-7 and the second pump chamber 3-13 compress the gas through the reciprocating motion of the piston 3-6 to form a negative pressure in the conveying pipeline, so that the alkali excites the fly ash colloid to generate flow potential energy in the conveying pipeline 3-18, thereby driving the liquid or slurry to be pumped through the pipeline. The pipeline connects the mixing device 2 and the pneumatic pump device 3 to transport the mixed alkali-activated fly ash colloid to the delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1. The ball valve 2-4 is used to control the flow of the alkali-activated fly ash colloid for mining, including starting, stopping and regulating flow operations.
[0113] Example 7
[0114] (1) Mix 3 parts of sodium hydroxide and 50 parts of fly ash and add them to 200 parts of water, then stir and mix in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which is filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate is tested for metal ions using an ICP tester, and the test results are: Si in the alkali-activated fly ash filtrate is 26729.91 mol / L, and Al is 2623.26 mol / L;
[0115] (2) adding alkali-activated fly ash, 0.2 parts of xanthan gum and 0.15 parts of carbomer to the dry material inlet 1-1 of the dry material proportioning unit, and stirring with the dry material agitator 1-3 to obtain dry material; adding the alkali-activated fly ash filtrate prepared in Example 3 to the water inlet 1-2 of the water material proportioning unit, and stirring with the water agitator 1-4 to obtain water material; monitoring the addition amount of alkali-activated fly ash in real time through the material quality controller 1-7, transmitting the addition amount of alkali-activated fly ash to the automatic proportioning system 1-9 for processing through the flow sensor 1-6 and the pressure sensor 1-5, and the automatic proportioning system 1-9 according to The preset proportion ratio and algorithm adjust the input amount of alkali-activated fly ash, xanthan gum and carbomer ingredients through flow sensors 1-6 to achieve accurate proportion requirements; the water material quality controller 1-8 can accurately control the amount of alkali-activated fly ash filtrate added to maintain the proportion accuracy, the pressure sensor 1-5 can monitor the pipeline pressure, ensure system safety, optimize fluid transportation, and the flow sensor 1-6 can measure the water material flow rate and accurately control the amount of water material added; at the same time, the pressure sensor 1-5 can work in conjunction with the quality controller to monitor pressure changes and adjust the flow rate to ensure the stability and accuracy of the flow rate;
[0116] The dry material and the water material are stirred in the stirring tank 2-1 by the stirring blade 2-3 connected to the electric stirrer 2-2 outside the stirring tank to obtain the alkali-activated fly ash colloid (the flow form of the alkali-activated fly ash colloid is as follows Figure 3 As shown), the obtained fly ash colloid is pumped into the goaf 4 through the pneumatic pump device 3; wherein, the electric mixer 2-2 provides power to drive the stirring blade 2-3 to rotate so that the materials are mixed evenly, and the ball valve 2-4 and the flow meter 2-5 are arranged on the connecting pipe between the stirring tank 2-1 and the conveying pipe 3-18 in the pneumatic diaphragm pump 3-1 to adjust the flow rate of the alkali-activated fly ash colloid;
[0117] The pneumatic pump device 3 includes a pneumatic diaphragm pump 3-1 and a compressed air system 3-17. The air outlet of the compressed air system is connected to the air supply port 3-2 of the pneumatic diaphragm pump 3-1 through an air pipe 3-16. A first pump chamber 3-7 and a second pump chamber 3-13 are arranged in the pneumatic diaphragm pump 3-1. The first pump chamber 3-7 and the second pump chamber 3-13 are connected through a first pump chamber connecting shaft 3-5. A piston 3-6 is arranged on the first chamber connecting shaft 3-5. The first pump chamber 3-7 and the second pump chamber 3-13 are also connected through a conveying pipe 3-18. A first pump chamber drive chamber 3-10 and a second pump chamber drive chamber 3-11 are respectively arranged in the first pump chamber 3-7 and the second pump chamber 3-13; a first pump chamber diaphragm 3-9 and a second pump chamber diaphragm 3-12 are respectively arranged in the first pump chamber drive chamber 3-10 and the second pump chamber drive chamber 3-11. The chamber drive chamber 3-11 is respectively connected to the air supply port 3-2 on the outside of the pneumatic diaphragm pump 3-1, and the automatic regulating valve 3-3 and the display device 3-4 are respectively arranged on the connecting pipes between the first pump chamber drive chamber 3-10, the second pump chamber drive chamber 3-11 and the air supply port 3-2. The automatic regulating valve 3-3 is used to adjust the air supply volume, and the display device 3-4 is used to display the opening of the regulating valve. The operation rate is adjusted by adjusting the automatic regulating valve 3-3; the compressed air system 3-17 compresses the air to the required pressure and provides stable compressed air for the pneumatic diaphragm pump 3-1. When the pneumatic force acts on the piston 3-6, the first pump chamber 3-7 and the second pump chamber 3-13 compress the gas through the reciprocating motion of the piston 3-6 to form a negative pressure in the conveying pipeline, so that the alkali excites the fly ash colloid to generate flow potential energy in the conveying pipeline 3-18, thereby driving the liquid or slurry to be pumped through the pipeline. The pipeline connects the mixing device 2 and the pneumatic pump device 3 to transport the mixed alkali-activated fly ash colloid to the delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1. The ball valve 2-4 is used to control the flow of the alkali-activated fly ash colloid for mining, including starting, stopping and regulating flow operations.
[0118] Example 8
[0119] (1) Mix 3 parts of sodium hydroxide and 50 parts of fly ash and add them to 200 parts of water, then stir and mix in a constant temperature water bath at 60°C for 48 hours to obtain an alkali-activated fly ash slurry, which is filtered to obtain an alkali-activated fly ash filtrate and alkali-activated fly ash. The alkali-activated fly ash filtrate is tested for metal ions using an ICP tester, and the test results are: Si in the alkali-activated fly ash filtrate is 26729.91 mol / L, and Al is 2623.26 mol / L;
[0120] (2) adding alkali-activated fly ash, 0.2 parts of xanthan gum and 0.15 parts of carbomer to the dry material inlet 1-1 of the dry material proportioning unit, and stirring with the dry material agitator 1-3 to obtain dry material; adding the alkali-activated fly ash filtrate prepared in Example 3 to the water inlet 1-2 of the water material proportioning unit, and stirring with the water agitator 1-4 to obtain water material; monitoring the addition amount of alkali-activated fly ash in real time through the material quality controller 1-7, transmitting the addition amount of alkali-activated fly ash to the automatic proportioning system 1-9 for processing through the flow sensor 1-6 and the pressure sensor 1-5, and the automatic proportioning system 1-9 according to The preset proportion ratio and algorithm adjust the input amount of alkali-activated fly ash, xanthan gum and carbomer ingredients through flow sensors 1-6 to achieve accurate proportion requirements; the water material quality controller 1-8 can accurately control the amount of alkali-activated fly ash filtrate added to maintain the proportion accuracy, the pressure sensor 1-5 can monitor the pipeline pressure, ensure system safety, optimize fluid transportation, and the flow sensor 1-6 can measure the water material flow rate and accurately control the amount of water material added; at the same time, the pressure sensor 1-5 can work in conjunction with the quality controller to monitor pressure changes and adjust the flow rate to ensure the stability and accuracy of the flow rate;
[0121] The dry material and the water material are stirred in the mixing tank 2-1 by the stirring blade 2-3 connected to the electric mixer 2-2 outside the mixing tank to obtain the alkali-activated fly ash colloid, and the obtained fly ash colloid is pumped into the goaf 4 through the pneumatic pump device 3; wherein the electric mixer 2-2 provides power to drive the stirring blade 2-3 to rotate so that the materials are mixed evenly, and the ball valve 2-4 and the flow meter 2-5 are arranged on the connecting pipe between the mixing tank 2-1 and the conveying pipe 3-18 in the pneumatic diaphragm pump 3-1 to adjust the flow rate of the alkali-activated fly ash colloid;
[0122] The pneumatic pump device 3 includes a pneumatic diaphragm pump 3-1 and a compressed air system 3-17. The air outlet of the compressed air system is connected to the air supply port 3-2 of the pneumatic diaphragm pump 3-1 through an air pipe 3-16. A first pump chamber 3-7 and a second pump chamber 3-13 are arranged in the pneumatic diaphragm pump 3-1. The first pump chamber 3-7 and the second pump chamber 3-13 are connected through a first pump chamber connecting shaft 3-5. A piston 3-6 is arranged on the first chamber connecting shaft 3-5. The first pump chamber 3-7 and the second pump chamber 3-13 are also connected through a conveying pipe 3-18. A first pump chamber drive chamber 3-10 and a second pump chamber drive chamber 3-11 are respectively arranged in the first pump chamber 3-7 and the second pump chamber 3-13; a first pump chamber diaphragm 3-9 and a second pump chamber diaphragm 3-12 are respectively arranged in the first pump chamber drive chamber 3-10 and the second pump chamber drive chamber 3-11. The chamber drive chamber 3-11 is respectively connected to the air supply port 3-2 on the outside of the pneumatic diaphragm pump 3-1, and the automatic regulating valve 3-3 and the display device 3-4 are respectively arranged on the connecting pipes between the first pump chamber drive chamber 3-10, the second pump chamber drive chamber 3-11 and the air supply port 3-2. The automatic regulating valve 3-3 is used to adjust the air supply volume, and the display device 3-4 is used to display the opening of the regulating valve. The operation rate is adjusted by adjusting the automatic regulating valve 3-3; the compressed air system 3-17 compresses the air to the required pressure and provides stable compressed air for the pneumatic diaphragm pump 3-1. When the pneumatic force acts on the piston 3-6, the first pump chamber 3-7 and the second pump chamber 3-13 compress the gas through the reciprocating motion of the piston 3-6 to form a negative pressure in the conveying pipeline, so that the alkali excites the fly ash colloid to generate flow potential energy in the conveying pipeline 3-18, thereby driving the liquid or slurry to be pumped through the pipeline. The pipeline connects the mixing device 2 and the pneumatic pump device 3 to transport the mixed alkali-activated fly ash colloid to the delivery pipeline 3-18 in the pneumatic diaphragm pump 3-1. The ball valve 2-4 is used to control the flow of the alkali-activated fly ash colloid for mining, including starting, stopping and regulating flow operations.
[0123] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An alkali-activated fly ash colloid grouting integrated device, characterized in that: It comprises an automatic proportioning device (1), a mixing device (2), and a pneumatic pump device (3) which are connected in sequence; The automatic proportioning device (1) comprises a dry material proportioning unit, a water material proportioning unit, a pressure sensor (1-5), a flow sensor (1-6) and an automatic proportioning system (1-9); The dry material proportioning unit comprises a dry material inlet (1-1), a dry material agitator (1-3) and a material quality controller (1-7); the water material proportioning unit comprises a water inlet (1-2), a water agitator (1-4) and a water material quality controller (1-8); The dry material inlet (1-1), the dry material agitator (1-3) and the material quality controller (1-7) are connected in sequence; The water inlet (1-2), the water agitator (1-4) and the water material quality controller (1-8) are connected in sequence; The mixing device (2) comprises a stirring tank (2-1); The dry material inlet (1-1) is connected to the stirring tank (2-1); the pressure sensor (1-5) and the flow sensor (1-6) are arranged on the connecting pipe between the dry material inlet (1-1) and the stirring tank (2-1); The water inlet (1-2) is connected to the stirring tank (2-1); the pressure sensor (1-5) and the flow sensor (1-6) are arranged on the connecting pipe between the water inlet (1-2) and the stirring tank (2-1); The pneumatic pump device (3) comprises a pneumatic diaphragm pump (3-1), an air supply port (3-2), an automatic regulating valve (3-3), a display device (3-4), a first pump chamber connecting shaft (3-5), a piston (3-6), a first pump chamber (3-7), a first pump chamber diaphragm (3-9), a first pump chamber drive chamber (3-10), a second pump chamber drive chamber (3-11), a second pump chamber diaphragm (3-12), a second pump chamber (3-13), a compressed air device (3-17) and a delivery pipeline (3-18); The stirring tank (2-1) is connected to a delivery pipeline (3-18) in a pneumatic diaphragm pump (3-1); The pneumatic diaphragm pump (3-1) is provided with a first pump chamber (3-7) and a second pump chamber (3-13); the first pump chamber (3-7) and the second pump chamber (3-13) are connected via a first pump chamber connecting shaft (3-5); a piston (3-6) is provided on the first chamber connecting shaft (3-5); a first pump chamber driving chamber (3-10) and a second pump chamber driving chamber (3-11) are provided on the first pump chamber (3-7) and the second pump chamber (3-13) respectively; a first pump chamber diaphragm (3-9) and a second pump chamber diaphragm (3-11) are provided in the first pump chamber driving chamber (3-10) and the second pump chamber driving chamber (3-11) respectively. The pump chamber diaphragm (3-12), the first pump chamber drive chamber (3-10) and the second pump chamber drive chamber (3-11) are respectively connected to the air supply port (3-2) outside the pneumatic diaphragm pump (3-1), the automatic regulating valve 3-3 and the display device 3-4 are arranged on the connecting pipe between the first pump chamber drive chamber (3-10), the second pump chamber drive chamber (3-11) and the air supply port (3-2); the air supply port (3-2) and the compressed air device (3-17) are connected through the first pipe (3-16); the first pump chamber (3-7) and the second pump chamber (3-13) are also connected through the delivery pipe (3-18).
2. The alkali-activated fly ash colloid grouting integrated device according to claim 1 is characterized in that: The mixing device (2) further comprises an electric stirrer (2-2), a stirring blade (2-3), a ball valve (2-4) and a flow meter (2-5); An electric stirrer (2-2) is arranged outside the stirring tank (2-1), a stirring blade (2-3) is arranged at the bottom of the stirring tank (2-1), and the stirring blade (2-3) is connected to the electric stirrer (2-2); The ball valve (2-4) and the flow meter (2-5) are arranged on a connecting pipe between the stirring tank (2-1) and a delivery pipe (3-18) in the pneumatic diaphragm pump (3-1).
3. The alkali-activated fly ash colloid grouting integrated process device according to claim 1 or 2, characterized in that: The pneumatic pump device (3) further comprises a one-way valve (3-8); The delivery pipeline (3-18) in the pneumatic diaphragm pump (3-1) is connected to the goaf (4) via a discharge pipeline; The one-way valve (3-8) is arranged on a delivery pipe (3-18) connecting the first pump chamber (3-7) and the second pump chamber (3-13); The pressure sensor (3-14) and the flow sensor (3-15) are arranged on a discharge pipe connecting a delivery pipe (3-18) in the pneumatic diaphragm pump (3-1) and the goaf (4).
4. A method for integrated grouting using the alkali-activated fly ash colloid grouting integrated device according to any one of claims 1 to 3, characterized in that: The following steps are involved: The dry material is added into the dry material proportioning unit, the water material is added into the water material proportioning unit, the dry material and the water material are mixed in a stirring tank (2-1) to obtain alkali-activated fly ash colloid, and the obtained alkali-activated fly ash colloid is grout-injected into the goaf 4 through a pneumatic pump device (3).
5. The alkali-activated fly ash colloid obtained by the alkali-activated fly ash colloid grouting integrated device according to any one of claims 1 to 3, characterized in that: The method is prepared by comprising the following raw materials in parts by weight: 0.1-0.5 parts of anionic polysaccharide macromolecular substance, 0.1-0.5 parts of macromolecular polymer, 10-30 parts of fly ash, 1-5 parts of alkali activator, 20-60 parts of water; The anionic polysaccharide macromolecular substance is xanthan gum or guar gum; The high molecular polymer is carbomer or welan gum.
6. The alkali-activated fly ash colloid according to claim 5, characterized in that: The alkaline activator is sodium hydroxide.
7. The alkali-activated fly ash colloid according to claim 6, characterized in that: The particle size of the fly ash is 0.01-200 μm.
8. The method for preparing alkali-activated fly ash colloid according to any one of claims 5 to 7, characterized in that: The following steps are involved: The alkali activator, fly ash and water are first mixed to obtain alkali activated fly ash filtrate and alkali activated fly ash through separation; Alkali-activated fly ash filtrate is added to the water-material proportioning unit, alkali-activated fly ash, anionic polysaccharide macromolecular substances and macromolecular polymers are added to the dry material proportioning unit, and the fly ash filtrate and the mixture of alkali-activated fly ash, anionic polysaccharide macromolecular substances and macromolecular polymers are mixed in a stirring tank (2-1) to obtain alkali-activated fly ash colloid.
9. The method for preparing alkali-activated fly ash colloid according to claim 8, characterized in that: The temperature of the first mixing is 40-70° C., and the time of the first mixing is 12-48 hours.