Induction heating compatible aluminum cooking utensil and manufacturing method thereof

By cold spraying the iron-based magnetic-conductive layer, aluminum bonding layer and enamel layer on aluminum cooking utensils, the problem that aluminum pots cannot be compatible with electromagnetic heating is solved, and the stability of electromagnetic induction heating and good bonding of the enamel layer is achieved. , improves the wear resistance and service life of the appliance.

CN118948115APending Publication Date: 2024-11-15朱颜明
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411258425.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-02
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing aluminum pots and pots are not compatible with electromagnetic heating, and the enamel coating is prone to internal stress caused by internal stress caused by ceramic collapse or cracking under electromagnetic heating conditions.

Method used

Cold spraying method is used to attach an iron-based magnetic-conducting layer of 0.08-0.5mm thick to the outer surface of the aluminum main body, followed by an aluminum bonding layer of 0.05-0.25mm thick, and an enamel layer is attached to the outer surface of the aluminum bonding layer to form an electromagnetic induction The heated aluminum enamel cooking utensil combines the enamel layer with the aluminum bonding layer through sintering to reduce internal stress.

Benefits of technology

The stability of aluminum cooking utensils under electromagnetic induction heating conditions and the good bonding of the enamel layer is achieved, the enamel layer is avoided, and the wear resistance and service life of the cooking utensils are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118948115A_ABST
    Figure CN118948115A_ABST
Patent Text Reader

Abstract

The invention provides an induction heating compatible aluminum cooking utensil and a manufacturing method thereof. The aluminum cooking utensil compatible with induction heating comprises an aluminum main body, and further comprises an iron-based magnetic conductive layer attached to the outer surface of the aluminum main body in a cold spraying mode; the aluminum bonding layer is attached to the outer surface of the iron-based magnetic conductive layer; the enamel layer is attached to the outer surface of the aluminum bonding layer; wherein the thickness of the iron-based magnetic conductive layer ranges from 0.08 mm to 0.5 mm, and the thickness of the aluminum bonding layer ranges from 0.05 mm to 0.25 mm. According to the induction heating compatible aluminum cooking utensil, the problem that in the prior art, an aluminum enamel pot cannot be compatible with induction heating can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cookware, and in particular to an aluminum cooking utensil compatible with induction heating and a manufacturing method thereof. Background Art

[0002] Aluminum materials have many advantages such as low specific gravity, high thermal conductivity, and easy processing and forming. They are ideal pot blank materials for cookware, especially non-stick cookware. For example, aluminum alloy materials such as grades 3003 and 3004 can be used to make aluminum stretched cookware, and aluminum alloy materials such as grade ADC12 can be used to make aluminum die-cast cookware. However, aluminum and aluminum alloy materials also have disadvantages such as soft surface, easy precipitation of aluminum ions, and no magnetic conductivity. Therefore, ordinary aluminum cookware has higher requirements for its surface treatment. The inner surface often needs to be provided with a non-stick layer and the outer surface often needs to be provided with a protective layer. In addition, ordinary aluminum cookware is not suitable for electromagnetic heating and cannot be used in electromagnetic heating appliances such as induction cookers.

[0003] Regarding the setting of protective layer on the outer surface, the industry has the method of forming an aluminum oxide protective film, and also the method of forming a coating using high temperature resistant silicone coating, ceramic coating and enamel coating. Among them, the enamel coating has relatively good wear resistance, high temperature resistance and decorative effect, and has a good application prospect; for the problem of not being suitable for electromagnetic heating, the industry has the scheme of setting a magnetic conductive composite bottom sheet or arc spraying iron layer on the bottom of aluminum pots. However, for the composite bottom scheme, due to the different materials, the bonding performance of the composite bottom sheet and the aluminum pot blank is usually poor, especially at high temperatures, due to the different thermal expansion coefficients, serious internal stress will be generated between the two; for the arc spraying scheme, due to the change of physical and mechanical properties of the material, internal stress will also be generated, and the porosity is generally greater than 5%; in addition, the temperature of sintering enamel and iron composite bottom sheet or iron layer to form iron enamel is above 850℃, which is higher than the melting point of aluminum pot blank, so it cannot be implemented on the iron composite bottom sheet or iron layer of aluminum pot blank. Therefore, it is usually difficult to provide an enamel coating on aluminum cookware that can currently be electromagnetically heated, and conversely, aluminum cookware that is provided with an enamel coating usually cannot be electromagnetically heated.

[0004] In view of this, it is necessary to propose a new technical solution to overcome the above-mentioned shortcomings. Summary of the invention

[0005] The present application provides an aluminum cooking utensil compatible with induction heating and a manufacturing method thereof, so as to solve the problem in the prior art that aluminum enamel pots are not compatible with induction heating.

[0006] To achieve the above-mentioned purpose, the present application adopts the following technical solution: an induction heating compatible aluminum cooking utensil, comprising an aluminum main body, the aluminum cooking utensil also comprising:

[0007] An iron-based magnetically conductive layer attached to the outer surface of the aluminum body by cold spraying;

[0008] an aluminum bonding layer attached to the outer surface of the iron-based magnetic conductive layer; and

[0009] an enamel layer attached to the outer surface of the aluminum bonding layer;

[0010] The thickness of the iron-based magnetic conductive layer is 0.08-0.5 mm, the porosity is not more than 2%, and the thickness of the aluminum bonding layer is 0.05-0.25 mm.

[0011] Optionally, the iron-based magnetic conductive layer has a thickness of 0.1-0.25 mm.

[0012] Optionally, the outer surface of the aluminum body is uneven.

[0013] Optionally, the diameter of the iron-based magnetic conductive layer is not less than 120 mm, and the unevenness of the outer surface of the aluminum body is not greater than 0.2 mm.

[0014] Optionally, the thickness of the aluminum bonding layer is 0.05-0.15 mm.

[0015] Optionally, the aluminum bonding layer is attached to the outer side of the iron-based magnetic conductive layer by cold spraying or aluminum wire arc spraying.

[0016] Optionally, the aluminum bonding layer covers the iron-based magnetic conductive layer.

[0017] Optionally, the iron-based magnetic conductive layer is formed on the bottom of the aluminum body, and the enamel layer is provided on the bottom and side of the aluminum cooking utensil;

[0018] The enamel layer at the bottom of the aluminum cooking utensil is combined with the aluminum bonding layer to form an aluminum enamel layer, and the enamel layer at the side of the aluminum cooking utensil is combined with the aluminum body to form an aluminum enamel layer.

[0019] Optionally, the enamel layer has a thickness of 15-90 μm.

[0020] Optionally, the enamel layer is sintered at 550-580°C.

[0021] Optionally, the inner surface of the aluminum body is provided with a metal reinforcement layer and a non-stick layer formed on the metal reinforcement layer.

[0022] Optionally, the metal strengthening layer has a thickness of 0.05-0.25 mm and a porosity of no more than 2%.

[0023] Optionally, the metal strengthening layer is formed on the aluminum body by cold spraying.

[0024] Optionally, the metal strengthening layer is made of iron, stainless steel or titanium.

[0025] Optionally, the non-stick layer is a ceramic non-stick layer.

[0026] Optionally, the material of the metal strengthening layer is iron and the thickness of the ceramic non-stick layer is 20-50 μm, or the material of the metal strengthening layer is stainless steel or titanium and the thickness of the ceramic non-stick layer is 5-40 μm.

[0027] The present application also provides a method for manufacturing an induction heating compatible aluminum cooking utensil, for manufacturing the induction heating compatible aluminum cooking utensil as described above, the method comprising:

[0028] An iron-based magnetic conductive layer is attached to the outer surface of the aluminum body by cold spraying;

[0029] An aluminum bonding layer is attached to the iron-based magnetic conductive layer;

[0030] attaching an enamel layer to the aluminum bonding layer; and

[0031] The enamel layer is sintered to combine with the aluminum bonding layer to form an aluminum enamel layer.

[0032] The induction heating compatible aluminum cooking utensil provided in the present application has a 0.08-0.5 mm thick iron-based magnetic conductive layer attached to the outer surface of the aluminum main body by cold spraying, a 0.05-0.25 mm thick aluminum bonding layer attached to the outer surface of the iron-based magnetic conductive layer, and an enamel layer attached to the outer surface of the aluminum bonding layer, thereby providing an aluminum enamel cooking utensil capable of electromagnetic induction heating, with low internal stress, good bonding of the enamel layer, and the enamel layer is not prone to chipping or cracking. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present application, rather than limiting the present application.

[0034] Figure 1 It is a schematic cross-sectional structure diagram of an embodiment of an aluminum cooking utensil compatible with induction heating of the present application.

[0035] Figure 2 It is a schematic diagram of a partially enlarged cross-sectional structure of the bottom wall of an embodiment of an aluminum cooking utensil compatible with induction heating in the present application.

[0036] Figure 3 It is a schematic diagram of a partially enlarged cross-sectional structure of the bottom wall of another embodiment of the induction heating compatible aluminum cooking utensil of the present application.

[0037] Figure 4It is a schematic diagram of a partially enlarged cross-sectional structure of a bottom wall in another embodiment of the induction heating compatible aluminum cooking utensil of the present application.

[0038] Figure 5a , 5b 5c is a schematic diagram of different pot types of aluminum cooking utensils compatible with induction heating in the present application.

[0039] Explanation of the reference numerals: 100, induction heating compatible aluminum cooking utensil; 11, side; 12, bottom; 1, aluminum body; 2, iron-based magnetic conductive layer; 3, aluminum bonding layer; 4, enamel layer; 5, metal reinforcement layer; 6, non-stick layer. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the present application will be further described in detail below with reference to the accompanying drawings. The components of the embodiments of the present application described and shown in the accompanying drawings can be arranged and designed in various configurations. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0041] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0042] Unless otherwise defined, the technical terms or scientific terms used in this patent document shall have the usual meanings understood by people with ordinary skills in the field to which this application belongs. The words "first", "second" and similar words used in the patent specification and claims of this application do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one", "one" or "the" do not indicate a quantitative limitation, but indicate the existence of at least one. Words such as "include" or "comprise" mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. "Center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly. It is only for the convenience of describing this application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application.

[0043] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0044] Some embodiments of the present application are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the features of the following embodiments can be combined with each other.

[0045] See also Figures 1 to 4 As shown, the present application discloses an induction heating compatible aluminum cooking utensil 100, comprising an aluminum body 1, an iron-based magnetic conductive layer 2 attached to the outer surface of the aluminum body 1 by cold spraying, an aluminum bonding layer 3 attached to the outer surface of the iron-based magnetic conductive layer 2, and an enamel layer 4 attached to the outer surface of the aluminum bonding layer 3; wherein the thickness of the iron-based magnetic conductive layer 2 is 0.08-0.5mm, and the thickness of the aluminum bonding layer 3 is 0.05-0.25mm.

[0046] The induction heating compatible aluminum cooking utensil 100 provided in the present application has an iron-based magnetic conductive layer 2 with a thickness of 0.08-0.5 mm attached to the outer surface of the aluminum main body 1 by cold spraying, an aluminum bonding layer 3 with a thickness of 0.05-0.25 mm attached to the outer surface of the iron-based magnetic conductive layer 2, and an enamel layer 4 attached to the outer surface of the aluminum bonding layer 3, thereby providing an aluminum enamel cooking utensil capable of electromagnetic induction heating, with low internal stress, good bonding of the enamel layer 4, and the enamel layer 4 is not prone to chipping or cracking.

[0047] The aluminum body 1 is a pot blank formed by stretching or die-casting of pure aluminum or aluminum alloy. For example, in some embodiments, the aluminum body 1 is a pot blank formed by stretching 3003 or 3004 aluminum alloy; in other embodiments, the aluminum body 1 is a pot blank formed by die-casting ADC12 aluminum alloy. The grade of the material used for the aluminum body 1 is not limited to the above examples, and it can also be other aluminum alloys.

[0048] The pot blank formed by the aluminum body 1 can be any possible pot shape, such as Figure 1 and Figure 5a , 5b 5c, it can be a flat pan, a round bottom pan, a spherical inner pot, a U-shaped pot, etc. It can be a frying pan suitable for stir-frying, a stew pot suitable for stewing, a soup pot suitable for boiling water, a rice cooker inner pot suitable for cooking, a pressure cooker pot suitable for pressure cooking, etc. The present application does not limit the specific pot type of the aluminum cooking utensil 100.

[0049] In order to enable the aluminum cooking utensil 100 to be electromagnetically heated, the outer surface of the aluminum body 1 is provided with an iron-based magnetic conductive layer 2. The iron-based magnetic conductive layer 2 is attached to the outer surface of the aluminum body 1 by cold spraying. Cold spraying is also called cold gas dynamic spraying. It uses compressed gas (such as nitrogen, helium and other gases) as an accelerating medium to accelerate metal particles to supersonic speed to drive the metal particles to collide with the substrate at a very high speed in the solid state, causing the particles to undergo strong plastic deformation and deposit on the substrate to form a coating. A new type of spraying technology. During the entire process of cold spraying, the metal particles are at a low temperature and are not melted. Moreover, since an inert gas is usually used for protection, the metal particle material is not melted or oxidized, and the original physical and chemical properties of the material are retained unchanged. The coating formed by cold spraying has a good bonding strength with the substrate; and since the coating material does not undergo a melting-solidification reshaping process, its internal stress is relatively small. The cold spraying process in one embodiment is as follows: an aluminum body 1 is used as a substrate, and its surface to be cold sprayed is roughened; the cold spraying equipment is started, and its equipment power is about 65KW, and nitrogen with a pressure of 8.5-10MPa, a flow rate of 2400L / Min, and a temperature of about 800-900°C is provided, driving the iron powder particles to impact the aluminum body 1 at a speed of 800-1000m / s, so that the iron powder particles undergo strong plastic deformation and are deposited on the aluminum body 1 to form the iron-based magnetic conductive layer 2. In one embodiment, the bonding strength of the formed iron-based magnetic conductive layer 2 with the aluminum body 1 is 55-80MP / cm 2 , the porosity is 1-2%.

[0050] The iron-based magnetic conductive layer 2 is formed by the cold spraying process of the material containing iron elements, and the material containing iron elements can be cast iron, stainless steel or other iron alloys. In one embodiment, the iron-based magnetic conductive layer 2 is attached to a partial area of ​​the outer surface of the aluminum body 1. For example, the aluminum cooking utensil 100 is a frying pan, and the iron-based magnetic conductive layer 2 is only attached to the bottom wall of the frying pan and is not arranged on the side wall, which can meet the induction heating with the flat induction cooker; for another example, the aluminum cooking utensil 100 is a round bottom pan, and the iron-based magnetic conductive layer 2 is attached to a partial area at the bottom of the round bottom pan, so as to meet the induction heating with the arc concave induction cooker. In another embodiment, the iron-based magnetic conductive layer 2 is attached to the entire area of ​​the outer surface of the aluminum body 1. For example, the aluminum cooking utensil 100 is an electromagnetically heated rice cooker or pressure cooker liner, and the iron-based magnetic conductive layer 2 is attached to almost the entire area of ​​the outer surface of the liner to achieve three-dimensional heating of the liner. That is, the setting area of ​​the iron-based magnetic conductive layer 2 can be set according to the specific pot type, and the present application does not limit the specific setting area of ​​the iron-based magnetic conductive layer 2 in some embodiments.

[0051] The thickness of the iron-based magnetic conductive layer 2 is 0.08-0.5mm. If the thickness of the iron-based magnetic conductive layer 2 is less than 0.08mm, the amount of heating generated by electromagnetic induction is small, resulting in low heating efficiency, which is difficult to meet the use requirements of the cooking utensil; if the thickness of the iron-based magnetic conductive layer 2 is greater than 0.5mm, the uniformity of thermal conductivity of the cooking utensil will be affected and the anti-deformation ability of the cooking utensil will be reduced. Although aluminum is a metal with good thermal conductivity, an overly thick iron-based magnetic conductive layer 2 causes a large amount of heat to be concentrated in a part of the aluminum body 1, causing the cooking utensil to be heated unevenly, affecting the cooking effect; at the same time, since the hardness of aluminum is relatively low and it is easy to deform due to heat, an overly thick iron-based magnetic conductive layer 2 will further reduce the anti-deformation ability of the aluminum body 1, making the area of ​​the aluminum body 1 where the iron-based magnetic conductive layer 2 is provided prone to high-temperature deformation. Moreover, an overly thick iron-based magnetic conductive layer 2 will also increase the weight and cost of the cooking utensil. Preferably, the thickness of the iron-based magnetic conductive layer 2 is 0.1-0.25mm. The porosity of the iron-based magnetic conductive layer 2 is not greater than 2%, so as to ensure that the iron-based magnetic conductive layer 2 is relatively dense and has better electromagnetic induction performance.

[0052] See also Figure 2 and Figure 3 As shown, in Figure 2 In the embodiment shown, the outer surface of the aluminum body 1 is generally a single plane or arc surface, on which the iron-based magnetic conductive layer 2, the aluminum bonding layer 3 and the enamel layer 4 are sequentially arranged. Figure 3 In the embodiment shown, the outer surface of the aluminum body 1 is uneven, and the outer surfaces of the iron-based magnetic conductive layer 2, the aluminum bonding layer 3 and the enamel layer 4 arranged thereon in sequence are also uneven. Figure 3 In the illustrated embodiment, by setting the outer surface of the aluminum body 1 to be uneven, a part of the internal stress can be absorbed during the process of thermal expansion and cooling contraction of the aluminum cooking utensil 100, thereby reducing the risk of cracking or porcelain collapse of each coating, especially the enamel layer 4. In one embodiment, the diameter of the iron-based magnetic conductive layer 2 is not less than 120 mm, so that the aluminum cooking utensil 100 has a larger sensing area. Due to the relatively large sensing area, the internal stress during thermal expansion and contraction is relatively large. The uneven setting of the outer surface of the aluminum body 1 helps to disperse the internal stress, wherein the amplitude of the unevenness is not greater than 0.2 mm. The amplitude of the unevenness refers to the vertical distance between the highest peak and the lowest peak. In this embodiment, the unevenness can be formed by extrusion or cutting, and it can be a smooth curved surface, a serrated surface or a relatively rough surface. The above-mentioned uneven outer surface can be set only in a part of the outer surface of the aluminum body 1, or in the whole area.

[0053] Please continue reading Figure 2 and Figure 3As shown, the aluminum bonding layer 3 is at least attached to the outer surface of the iron-based magnetic conductive layer 2. In one embodiment, the aluminum bonding layer 3 covers the iron-based magnetic conductive layer 2. The setting of the aluminum bonding layer 3 is suitable for the enamel layer 4 to be sintered with the aluminum bonding layer 3 at a lower sintering temperature to form aluminum enamel. In some embodiments, the thickness of the aluminum bonding layer 3 is 0.05-0.25 mm. When the thickness of the aluminum bonding layer 3 is less than 0.05 mm, the bonding performance of the enamel layer 4 is insufficient, because during the sintering process of the enamel layer 4 and the aluminum bonding layer 3, the overly thin aluminum bonding layer 3 does not cover the iron-based magnetic conductive layer 2 enough, which makes it easy for the enamel layer 4 to contact the iron-based magnetic conductive layer 2. The contact between the enamel layer 4 and the iron-based magnetic conductive layer 2 greatly increases the difficulty of bonding. It cannot form iron enamel when sintered at the sintering temperature of 550-580°C for forming aluminum enamel. The sintering temperature of enamel and iron-based material must be above 850°C to combine into iron enamel, which is impossible on aluminum cooking utensils 100. When the thickness of the aluminum bonding layer 3 is greater than 0.25 mm, the iron-based magnetic conductive layer 2 therein is affected by the excessive thickness, which affects the electromagnetic induction and the efficiency of induction heating. Preferably, the thickness of the aluminum bonding layer is 0.05-0.15 mm. The aluminum bonding layer 3 is attached to the outer side of the iron-based magnetic conductive layer 2 by cold spraying or aluminum wire arc spraying. The aluminum wire arc spraying process uses two aluminum wires with positive and negative charges respectively, which contact each other to generate an arc. The high temperature of the arc instantly melts the aluminum wire, and the molten aluminum is atomized into tiny particles by high-speed airflow. These atomized aluminum particles are accelerated by the high-speed airflow and sprayed onto the surface of the target substrate to accumulate and solidify on the surface of the substrate to form a relatively uniform and rough coating.

[0054] In one embodiment, the iron-based magnetic conductive layer 2 is formed at the bottom of the aluminum main body 1, the aluminum bonding layer 3 covers the iron-based magnetic conductive layer 2, and the enamel layer 4 is provided at the bottom 12 and the side 11 of the aluminum cooking utensil 100; wherein the enamel layer 4 located at the bottom 12 of the aluminum cooking utensil is combined with the aluminum bonding layer 3 to form an aluminum enamel layer, and the enamel layer 4 located at the side 11 of the aluminum cooking utensil is combined with the aluminum main body 1 to form an aluminum enamel layer. The thickness of the enamel layer 4 is 15-90 μm. When the thickness of the enamel layer 4 is less than 15 μm, its strength and wear resistance are insufficient, and it is difficult to play a good wear-resistant and decorative role. When its thickness is greater than 90 μm, the electromagnetic induction of the iron-based magnetic conductive layer 2 inside it is affected, resulting in a decrease in thermal efficiency, and at the same time, the weight of the cooking utensil is increased, and the cost is increased. In the present application, the enamel layer 4 is either sintered with the aluminum body 1 or sintered with the aluminum bonding layer 3, and is aluminum enamel sintered at 550-580°C.

[0055] See also Figure 4As shown, in one embodiment, the inner surface of the aluminum body 1 is provided with a metal reinforcement layer 5 and a non-stick layer 6 formed on the metal reinforcement layer 5. The metal reinforcement layer 5 is provided so that the non-stick layer 6 has a solid bonding base, which can improve the bonding strength and wear resistance and impact resistance of the non-stick layer 6. In some embodiments, the thickness of the metal reinforcement layer 5 is 0.05-0.25 mm, and the porosity is not greater than 2%. The metal reinforcement layer 5 is formed on the aluminum body 1 by cold spraying, and the material of the metal reinforcement layer 5 is iron, stainless steel or titanium. In some embodiments, the non-stick layer 6 is a ceramic non-stick layer. A metal reinforcement layer with a thickness of 0.05-0.25 mm is first provided on the inner surface of the formed aluminum body 1, and then the ceramic non-stick layer is coated, so that the ceramic non-stick layer can be set thinner to reduce its internal stress, while improving the wear resistance and impact resistance of the ceramic non-stick layer. In one embodiment, the inner surface treatment process of the aluminum body 1 is as follows: first, the inner and outer surfaces of the formed aluminum body 1 are cleaned, washed and sandblasted to expose fresh aluminum alloy materials with a certain degree of roughness, and then the metal strengthening layer 5 is set by cold spraying, and then the ceramic non-stick layer is coated on the surface of the metal strengthening layer 5. Before coating the ceramic non-stick layer, sandblasting can also be performed. Sandblasting can enhance the bonding force between the ceramic non-stick layer and the metal strengthening layer 5. In one embodiment, the material of the metal strengthening layer 5 is iron, and the thickness of the ceramic non-stick layer is set to 20-50 μm. It is relatively thick so that it has good anti-rust performance to protect the metal strengthening layer 5. In another embodiment, the material of the metal strengthening layer 5 is stainless steel or titanium, and the thickness of the ceramic non-stick layer can be relatively thin, set to 5-40 μm. Because the ceramic non-stick layer has excellent wear resistance, under the premise of satisfying the anti-rust of the metal strengthening layer 5 material, the thin thickness of the ceramic non-stick layer is less likely to cause the coating to collapse or crack due to internal stress.

[0056] See also Figure 5a , 5b As shown in 5c, the aluminum cooking utensil 100 provided in the present application can be a flat pan, a round bottom pan, a spherical inner pot, a U-shaped pot, etc. Figure 5c As shown, the position where the iron-based magnetic conductive layer 2 and the aluminum bonding layer 3 are required to be set on the aluminum main body 1 can be concave, and the concave depth is equivalent to the sum of the thicknesses of the iron-based magnetic conductive layer 2 and the aluminum bonding layer 3 to be set, so as to realize the iron-based magnetic conductive layer 2 and the aluminum bonding layer 3 being set on the aluminum main body 1 in an embedded manner, and then the enamel layer 4 is set to cover the outer surface of the aluminum main body 1 and the aluminum bonding layer 3.

[0057] The present application also provides a method for manufacturing an induction heating compatible aluminum cooking utensil 100, which is used to manufacture the induction heating compatible aluminum cooking utensil 100 as described above, the method comprising: attaching an iron-based magnetic conductive layer 2 on the outer surface of an aluminum main body 1 by cold spraying; attaching an aluminum bonding layer 3 on the iron-based magnetic conductive layer 2; attaching an enamel layer 4 on the aluminum bonding layer 3; and sintering so that the enamel layer 4 is combined with the aluminum bonding layer 3 to form an aluminum enamel layer. The enamel layer 4 is also partially located on the outer surface of the aluminum main body 1. During the above sintering process, the enamel layer 4 located on the outer surface of the aluminum main body 1 is combined with the aluminum main body 1 to form an aluminum enamel layer. The contents not described in the manufacturing method provided in the present application can be understood by referring to the above description of the induction heating compatible aluminum cooking utensil 100.

[0058] In one embodiment, a method for manufacturing an induction heating compatible aluminum cooking utensil comprises the following steps:

[0059] Step S1, cleaning the formed pot body by decontamination and degreasing, and then performing high-pressure sandblasting on the outer surface of the bottom 12 of the pot body to increase the surface area of ​​the outer surface of the bottom 12 of the pot body, and also to form a roughening effect on the outer surface of the bottom 12 of the pot body, thereby effectively increasing the bonding strength of the iron-based magnetic conductive layer 2 in the next process, and the outer surface of the bottom 12 of the pot body is a smooth surface;

[0060] Step S2, cold spraying iron powder on the electromagnetic heating area of ​​the bottom 12 of the pot body to form an iron-based magnetic conductive layer 2 for magnetic conductivity, so as to ensure that the aluminum enamel pot can be heated by electromagnetic induction;

[0061] Step S3, coating the aluminum alloy or pure aluminum on the outer surface of the iron-based magnetic conductive layer 2 by cold spraying to form an aluminum bonding layer 3, and the coating range of the aluminum bonding layer 3 covers the entire iron-based magnetic conductive layer 2 and extends outward to the periphery of the iron-based magnetic conductive layer 2;

[0062] Step S4, spraying aluminum enamel on the surface of the pot body and covering the aluminum bonding layer 3, then sintering and forming the aluminum enamel layer, and utilizing the fact that the ductility of the aluminum bonding layer 3 is greater than that of the iron-based magnetic conductive layer 2 to disperse the stress between each other; at the same time, since the iron-based magnetic conductive layer 2 is formed by powder cold spraying deposition, compared with the iron-based substrate covering in the prior art, the thermal stress can be dispersed between the powder particles, thereby better ensuring the bonding strength of the aluminum enamel layer on the surface of the pot body.

[0063] According to GB / T 11419-2008, the method for determining the temperature deformation resistance of enamel cookware, aluminum enamel cookware needs to undergo temperature resistance test or hot and cold shock test before leaving the factory. Since the temperature of open flame cookware after dry burning is generally between 300 and 450℃, the actual test adopts a test temperature of at least 350℃ and is repeated at least 10 times according to the GB / T 11419-2008 method to determine whether the aluminum enamel layer has abnormal phenomena such as falling off or cracking.

[0064] The ductility of the aluminum bonding layer 3 is greater than that of the iron-based magnetic conductive layer 2, so as to ensure that the aluminum bonding layer 3 with high ductility can adaptively deform and fill the arc angle formed at the outer edge of the iron-based magnetic conductive layer 2 with low ductility, so as to effectively eliminate the stress fault formed by the aluminum enamel layer at the outer edge of the iron-based magnetic conductive layer 2, release the corresponding stress, and further ensure the bonding strength of the aluminum enamel layer on the surface of the pot body.

[0065] At 20°C, the thermal expansion coefficient of iron is 12.2×10 -6 / K, the thermal expansion coefficient of aluminum is 23.2×10 -6 / K and the thermal expansion coefficient of the aluminum enamel layer is 69.6 to 70.8×10 -6 / K, it can be seen that the thermal expansion coefficient of iron is smaller than that of aluminum, and the thermal expansion coefficient of the aluminum enamel layer is larger than that of iron and aluminum, respectively.

[0066] The arc angle design at the connection between the bottom 12 of the pot body and the pot body is used to avoid the formation of a stress fault with concentrated thermal stress between the iron-based magnetic conductive layer 2 and the pot body, so as to release the corresponding stress, thereby enhancing the bonding strength of the aluminum enamel layer on the surface of the pot body. By utilizing the fact that the ductility of the iron-based magnetic conductive layer 2 is lower than that of the aluminum bonding layer 3, the stress between each other is dispersed, thereby ensuring the bonding strength of the aluminum enamel layer 4 on the surface of the pot body, thereby ensuring that the aluminum enamel layer does not fall off during daily use or after sintering. It is not only suitable for heating methods such as open flames and induction cookers, but also has a good overall appearance of the aluminum enamel cookware, and can also ensure sufficient service life, wear resistance and corrosion resistance, and at the same time meets the relevant provisions of the standard document GB / T 32147-2015.

[0067] Of course, in other embodiments, the coating ranges of the aluminum bonding layer 3 and the iron-based magnetic conductive layer 2 may also overlap or substantially overlap.

[0068] In step S1 of the preferred embodiment, the surface roughness of the outer surface of the bottom 12 of the pot body after high-pressure sandblasting surface treatment is 4.5 to 5.5 μm, which greatly increases the surface area of ​​the bottom 12 of the pot body. High-pressure sandblasting is used to make the rough surface after sandblasting form a snowflake-like roughening effect, thereby better enhancing the bonding strength between coatings.

[0069] In a specific embodiment, when the cold spray diameter of the iron-based magnetic conductive layer 2 is less than 150 mm, high-pressure sandblasting is directly performed; when the cold spray diameter of the iron-based magnetic conductive layer 2 exceeds 150 mm, embossing is performed on the electromagnetic heating area of ​​the bottom 12 of the pot body that has not been subjected to high-pressure sandblasting surface treatment to ensure that a concave and convex surface is formed on the bottom of the pot body; of course, in other embodiments, during casting, the electromagnetic heating area at the bottom of the pot body is pulled and die-cast into a concave groove through a mold to increase the surface area.

[0070] Whether it is embossing, or molded by mold pulling and die casting, the surface concave-convex value of the bottom 12 of the pot body is 0.1 to 0.2 mm, and then the total surface area of ​​the bottom 12 of the pot body is increased again by sandblasting. Compared with the bottom 12 of the pot body with the same diameter without concave-convex surface and sandblasting roughening treatment, the total surface area of ​​the bottom 12 of the pot body is increased by 3 to 5 times, that is, the total surface area of ​​the bottom 12 of the pot body is further increased, thereby further enhancing the adhesion and bonding strength of the iron-based magnetic conductive layer 2 on the surface of the bottom 12 of the pot body.

[0071] In step S2 of the preferred embodiment, an iron-based magnetic conductive layer 2 with a thickness of 100 to 200 μm, such as an iron-based magnetic conductive layer 2 with a thickness of 0.12 mm, 0.15 mm or 0.18 mm, is formed by a supersonic cold spraying process, and the spraying diameter of the iron-based magnetic conductive layer 2 is 120 to 250 mm.

[0072] In this embodiment, the air chamber pressure of the supersonic cold spraying of the iron-based magnetic conductive layer 2 is 4.6±0.5MPa, the powder feeding pressure is 4.7±0.5Mpa, the air chamber temperature is 750 to 800°C, the distance between the cold spray gun mouth and the pot body is 20 to 30mm, and the powder feeding amount is 10 to 200g / min. At this time, the cold spraying process is used to use compressed gas as an accelerating airflow to drive the iron-based powder particles or iron powder (iron powder particle size is between 1 and 50μm) to flow, and in the lower spraying temperature range from room temperature to 200°C at the spray gun mouth, at a supersonic jet speed of 800 to 1200m / s, and the iron The powder particles collide with the outer surface of the bottom 12 of the pot body in a softened state, and cooperate with the bottom 12 of the pot body to form a magnetic iron-based magnetic layer 2 through the setting of concave and convex surfaces and sandblasting roughening, so that the iron powder particles undergo strong plastic deformation, and then are deposited on the outer surface of the bottom 12 of the pot body to form a magnetic iron-based magnetic layer 2, thereby ensuring that the film thickness of the iron-based magnetic layer 2 is uniform, the coating is dense, and the porosity is low. It can also ensure that the compressive stress and thermal stress between the coatings formed by the accumulation of iron powder during cold spraying are low, so as to ensure the adhesion of the subsequent aluminum enamel layer 4, and also avoid the aluminum enamel layer 4 from falling off and cracking due to stress concentration.

[0073] In addition, the iron-based magnetic conductive layer 2 is formed by supersonic cold spraying, which has little thermal impact on the matrix formed by the bottom 12 of the pot body and the iron powder particles, thereby avoiding abnormal phenomena such as oxidation, burning, phase change and organizational change of the iron powder during spraying. Moreover, during the spraying process, the impact of subsequent iron powder particles has a compacting effect on the initial coating on the substrate. At the same time, there is no volume shrinkage of the coating or film during the process of hot coating or thermal spraying to form the coating, thereby ensuring low porosity and bubble rate, and effectively preventing the corrosive medium from penetrating into the bonding surface of the coating and the substrate to cause galvanic corrosion.

[0074] When the cold spray diameter of the iron-based magnetic conductive layer 2 exceeds 150 mm, the electromagnetic heating zone 13 at the bottom of the pot body is provided with a concave-convex surface, and the depth of the concave-convex surface is not greater than 0.2 mm to ensure the high adhesion of the iron-based magnetic conductive layer 2.

[0075] In step S3 of the preferred embodiment, the aluminum bonding layer 3 having a thickness of 5 to 15 μm is formed by cold spraying aluminum or aluminum alloy powder.

[0076] In this embodiment, the air chamber pressure of the cold spraying of the aluminum bonding layer 3 is 3.5±0.5MPa, the powder feeding pressure is 3.6±0.5MPa, the air chamber temperature is 550 to 600°C, the distance between the cold spray gun mouth and the pot body is 20 to 30mm, and the powder feeding amount is 10 to 100g / min, so as to ensure that the film thickness of the aluminum bonding layer 3 is uniform, and the steps or arc corners formed on the outer edge of the iron-based magnetic conductive layer 2 are effectively filled, and the transition is smooth, so as to achieve low and dispersed internal stress between each other, thereby ensuring that the aluminum bonding layer 3 and the aluminum enamel layer here will not crack or collapse due to hot and cold shock tests.

[0077] In step S4 of the preferred embodiment, the enamel layer 4 is sprayed on the bottom 12 of the pot body and the outer side of the pot body, and then sintered. The specific sintering process is as follows: the sintering temperature of the aluminum enamel is 550 to 580°C, the sintering time is at least 5 minutes, and the thickness of the aluminum enamel layer formed by sintering is 20 to 80 μm, so that an enamel effect with good appearance is obtained. At the same time, the overall performance of the aluminum enamel cookware is more superior, such as wear resistance and corrosion resistance.

[0078] In a specific embodiment, the pot body sprayed with the aluminum bonding layer 3 is firstly lightly polished to remove abnormal protrusions such as edges, corners, burrs, etc., and then the aluminum enameling process is carried out.

[0079] Compared with the prior art, the aluminum enamel cookware composed of the iron-based magnetic conductive layer 2 formed by cold spraying and the aluminum bonding layer 3 formed by cold spraying in this embodiment can achieve good magnetic conductivity, thermal stress resistance, bonding strength and dispersed low-pressure stress. Moreover, the bonding strength between each adhesion layer and between each adhesion layer and the substrate (i.e., the pot body) is significantly improved, and abnormal phenomena such as bubbles, cracking, and shedding that exist in the prior art will not occur.

[0080] In addition, through comparative experiments, that is, in hot and cold shock tests or heat resistance tests between room temperature and high temperature of 350°C, after the aluminum enamel cookware samples of this embodiment were repeatedly tested 35-40 times, no cracks were found between the iron-based magnetic conductive layer 2 and the pot body (or substrate), and between the aluminum enamel layer 4 and the aluminum bonding layer 3 formed by cold spraying.

[0081] At the same time, compared with the aluminum enamel cookware formed by directly performing the aluminum enamel process on the newly formed pot body in the prior art, since the iron-based magnetic conductive layer 2 of iron-based material is added between the pot body and the aluminum enamel layer, it can play a strengthening role, thereby achieving the effect of significantly enhancing the hardness of the outermost aluminum enamel layer. Therefore, the wear resistance of the aluminum enamel cookware of this embodiment is further enhanced.

[0082] In addition, since the iron-based magnetic conductive layer 2 and the aluminum bonding layer 3 of the present embodiment effectively absorb the thermal stress of the pot body, the thermal deformation rate or the flatness (i.e. the amount of bending area to the inside) of the aluminum enamel cookware of the present embodiment in the heating state is much lower than the standard value specified in GB / T 32147-2015, and the actual test data of the heat shock resistance and bottom firmness of the bottom of the aluminum enamel cookware of the present embodiment are also significantly better than the standard values ​​of GB / T 32147-2015. Please refer to the following Table 1 for specific comparison data.

[0083] Table 1

[0084]

[0085] In some embodiments of the present application, the connection between the bottom 12 of the pot body and the pot body is processed with an arc angle through a designed molding mold, such as using a preset R-angle casting mold to cast a pot body with an R angle, so as to avoid the obvious fault between the outer edge of the iron magnetic conductive sheet and the bottom of the aluminum cookware in the prior art. Such a preset arc angle can ensure that the stress formed between the iron-based magnetic conductive layer 2 and the pot body during high-temperature sintering or dry burning by the user is released toward the direction of the pot body or the pot mouth.

[0086] Of course, in other embodiments, such as the bottom of a frying pan, when the iron-based magnetic conductive layer 2 extends to the connection between the bottom 12 of the pan body and the side wall of the pan body, this position also needs to be arc-angled to eliminate obvious faults, that is, to avoid excessive stress concentration at the fault and inability to release it.

[0087] From the above description of the specific embodiments, it can be known that the induction heating compatible aluminum cooking utensil 100 provided in the present application has an iron-based magnetic conductive layer 2 with a thickness of 0.08-0.5 mm attached to the outer surface of the aluminum body 1 by cold spraying, an aluminum bonding layer 3 with a thickness of 0.05-0.25 mm attached to the outer surface of the iron-based magnetic conductive layer 2, and an enamel layer 4 attached to the outer surface of the aluminum bonding layer 3, thereby providing an aluminum enamel cooking utensil 100 capable of electromagnetic induction heating, with low internal stress, good bonding of the enamel layer 4, and the enamel layer 4 is not prone to chipping or cracking.

[0088] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. An induction heating compatible aluminum cooking utensil comprising an aluminum body, It is characterized in that The aluminum cooking utensil further comprises: An iron-based magnetically conductive layer attached to the outer surface of the aluminum body by cold spraying; an aluminum bonding layer attached to the outer surface of the iron-based magnetic conductive layer; and an enamel layer attached to the outer surface of the aluminum bonding layer; Wherein, the thickness of the iron-based magnetic conductive layer is 0.08-0.5 mm, and the thickness of the aluminum bonding layer is 0.05-0.25 mm.

2. The induction heating compatible aluminum cooking utensil of claim 1, It is characterized in that The thickness of the iron-based magnetic conductive layer is 0.1-0.25 mm, and the porosity is not greater than 2%. The thickness of the aluminum bonding layer is 0.05-0.15 mm.

3. The induction heating compatible aluminum cooking utensil of claim 1, It is characterized in that The outer surface of the aluminum body is uneven.

4. The induction heating compatible aluminum cooking utensil of claim 3, It is characterized in that The diameter of the iron-based magnetic conductive layer is not less than 120 mm, and the unevenness of the outer surface of the aluminum body is not greater than 0.2 mm.

5. The induction heating compatible aluminum cooking utensil of claim 4, It is characterized in that The aluminum bonding layer is attached to the outer side of the iron-based magnetic conductive layer by cold spraying or aluminum wire arc spraying.

6. The induction heating compatible aluminum cooking utensil of claim 1, It is characterized in that The iron-based magnetic conductive layer is formed on the bottom of the aluminum body, and the enamel layer is provided on the bottom and side of the aluminum cooking utensil; The enamel layer at the bottom of the aluminum cooking utensil is combined with the aluminum bonding layer to form an aluminum enamel layer, and the enamel layer at the side of the aluminum cooking utensil is combined with the aluminum body to form an aluminum enamel layer.

7. The induction heating compatible aluminum cooking utensil of claim 1 or 6, It is characterized in that The thickness of the enamel layer is 15-90 μm.

8. The induction heating compatible aluminum cooking utensil of claim 1 or 6, It is characterized in that The enamel layer is sintered at 550-580°C.

9. The induction heating compatible aluminum cooking utensil of claim 1, It is characterized in that The inner surface of the aluminum body is provided with a metal reinforcement layer and a non-stick layer formed on the metal reinforcement layer.

10. The induction heating compatible aluminum cooking utensil of claim 9, It is characterized in that The thickness of the metal strengthening layer is 0.05-0.25 mm, and the porosity is not more than 2%.

11. The induction heating compatible aluminum cooking utensil of claim 9, It is characterized in that The metal reinforcement layer is formed on the aluminum body by cold spraying.

12. The induction heating compatible aluminum cooking utensil of claim 11, It is characterized in that The material of the metal strengthening layer is iron, stainless steel or titanium.

13. The induction heating compatible aluminum cooking utensil of claim 9, It is characterized in that The non-stick layer is a ceramic non-stick layer.

14. The induction heating compatible aluminum cooking utensil of claim 13, It is characterized in that The material of the metal strengthening layer is iron and the thickness of the ceramic non-stick layer is 20-50 μm, or the material of the metal strengthening layer is stainless steel or titanium and the thickness of the ceramic non-stick layer is 5-40 μm.

15. A method for manufacturing an induction heating compatible aluminum cooking utensil, for manufacturing the induction heating compatible aluminum cooking utensil as claimed in any one of claims 1 to 14, It is characterized in that The method comprises: An iron-based magnetic conductive layer is attached to the outer surface of the aluminum body by cold spraying; An aluminum bonding layer is attached to the iron-based magnetic conductive layer; attaching an enamel layer to the aluminum bonding layer; and The enamel layer is sintered to bond with the aluminum bonding layer to form an aluminum enamel layer.

Citation Information

Cited By

  • Induction-compatible cooking vessel and method for manufacturing an induction-compatible cooking vessel

    DE102024138750A1