Lipoic acid-based deep eutectic supramolecular polymer adhesive as well as preparation method and application thereof

The deep eutectic supramolecular polymer adhesive is formed by mixing and heating of lipoic acid and sodium lipoate, which solves the problem of unstable lipoic acid-based adhesive after the temperature drops, and achieves stable adhesion and biological activity release in the body, promoting the The effect of wound healing is better than traditional sutures.

CN118949109AActive Publication Date: 2024-11-15TIANJIN UNIV

Patent Information

Application Number
CN202310538371.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

The existing lipoic acid-based adhesives are unstable after the temperature is reduced or the solvent is volatile, and the biocompatibility and tissue adhesion are insufficient, which limits their application in the biomedical field, especially in vivo use.

Method used

By mixing lipoic acid and sodium lipoate at different mass ratios and performing one-step heating and melting, a lipoic acid-based deep eutectic supramolecular polymer binder is formed, and the melting temperature is reduced by strong hydrogen bonds and the deep eutectic phenomenon is achieved, forming a stable supramolecular polymers enhance adhesion and biocompatibility.

Benefits of technology

Supramolecular polymers that remain stable at room temperature are achieved, which enhances adhesion to various substrates and releases of bioactive small molecules, promotes wound healing, and is better than traditional surgical sutures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949109A_ABST
    Figure CN118949109A_ABST
Patent Text Reader

Abstract

The invention discloses a lipoic acid-based deep eutectic supramolecular polymer adhesive as well as a preparation method and application thereof. The lipoic acid-based deep eutectic supramolecular polymer adhesive can be obtained by further heating a mixture of lipoic acid and lipoic acid salt. In the heating process, multiple strong hydrogen bonds are formed between carboxyl at the tail end of lipoic acid and carboxylate at the tail end of sodium lipoate to promote the mixture to generate a deep eutectic phenomenon, and the powder state of the mixture is converted into a viscous liquid state. After the mixture is co-melted, sulfur-containing five-membered rings of the lipoic acid and the sodium lipoate can be subjected to spontaneous ring opening and copolymerization to form a supramolecular polymer. The adhesive provided by the invention can realize stable and high-strength adhesion to various matrixes, can be used as a hot melt adhesive, and has anti-inflammatory, bactericidal and antioxidant effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to the preparation and application research of a lipoic acid-based deep eutectic supramolecular polymer adhesive. Background Art

[0002] Lipoic acid is often used to prepare adhesives due to the carboxyl radicals at the end. Lipoic acid monomers undergo spontaneous ring opening to form polylipoic acid when heated. However, due to the presence of thiol radicals at the end of the formed polylipoic acid, polylipoic acid is unstable when the temperature is reduced or the solvent evaporates, and reversible spontaneous depolymerization occurs, which then turns into polylipoic acid oligomers or lipoic acid small molecules, and the final product is an opaque semi-crystalline state, and the product does not have any tissue adhesion. Although it is currently reported that the stability of polylipoic acid can be achieved by introducing multi-double bond monomers, multivalent metal ions, and ionic liquids into the lipoic acid system, the biocompatibility of the obtained materials is significantly reduced, which is not suitable for application in the biomedical field. In addition, the tight cross-linking and natural hydrophobic properties of lipoic acid molecules in these materials make it difficult to achieve the release of small molecules, and therefore, the biological activity of lipoic acid monomers is greatly buried. In addition, the melting temperature of lipoic acid, which is much higher than body temperature, also limits its application in vivo.

[0003] Epidermal damage often occurs in daily life, and severe cases often require suturing. However, traditional surgical sutures are not only time-consuming and non-degradable, but also cause secondary damage to the tissue, increasing the patient's pain. After the surgical sutures are sutured, the wound healing part often leaves scars, which increases the patient's mental stress. In order to overcome these defects of traditional surgical sutures, biological tissue adhesives are designed to replace surgical sutures to accelerate wound healing. However, traditional tissue adhesives, such as biological glue or fibrin glue, have low adhesion strength to tissues and cannot effectively seal skin wounds. Although cyanoacrylate-based adhesives can achieve rapid and high-strength adhesion to tissues, the hardening of the adhesive after adhesion and the toxic degradation products are easy to cause infection at the wound site, which is not conducive to tissue healing. Therefore, it is very urgent to develop tissue adhesives with good biocompatibility and excellent tissue adhesion. Summary of the invention

[0004] The object of the present invention is to overcome the deficiencies of the prior art, to provide a thioctic acid-based deep eutectic supramolecular polymer adhesive and its preparation method and application, with thioctic acid monomer and sodium thioctic acid monomer as raw materials, by fully mixing and grinding the two powders at different mass ratios and then heating and melting to obtain a thioctic acid-based hot melt adhesive. In this adhesive, the strong electron-withdrawing properties of the carboxylate structure at the end of sodium thioctic acid allow it to form a strong hydrogen bond with the carboxyl group at the end of thioctic acid, so it can effectively reduce the melting temperature of the mixture, and by regulating the ratio between the two, the melting temperature of the mixture is reduced to close to body temperature, thereby realizing in vivo application. This is completely different from the aqueous solution reaction recorded in the previous invention application "A Sodium Polythioate-Polythioic Acid Composite Adhesive Patch and Its Preparation Method and Application" (Application No. 2023103748352, Application Date April 10, 2023) of this research group, and the obtained products and performance are also completely different.

[0005] The technical purpose of the present invention is achieved through the following technical solutions.

[0006] A lipoic acid-based deep eutectic supramolecular polymer adhesive and a preparation method thereof. Lipoic acid and sodium lipoate are mixed and ground, heated to melt, and then cooled to room temperature of 20-25 degrees Celsius to obtain the lipoic acid-based deep eutectic supramolecular polymer adhesive.

[0007] The mass ratio of lipoic acid to sodium lipoate is (0.5-3):1, preferably (0.5-2):1.

[0008] The melting temperature is 180-42 degrees Celsius, preferably 180-49 degrees Celsius.

[0009] The invention discloses an application of the lipoic acid-based deep eutectic supramolecular polymer adhesive in preparing wound adhesion / repair materials.

[0010] During the preparation, the raw materials of lipoic acid and sodium lipoate and the product lipoic acid-based deep eutectic supramolecular polymer adhesive are sterilized, such as by ethylene oxide sterilization, before being used or tested in vivo.

[0011] The supramolecular polymer adhesive of the present invention can be obtained by heating a mixture of thioctic acid and thioctic acid salt (sodium thioate) in one step. During the heating process, the carboxyl group at the end of thioctic acid and the carboxylate structure at the end of sodium thioate promote the deep eutectic phenomenon of the mixture by forming multiple strong hydrogen bonds, and the powder state of the mixture is converted into a viscous liquid state. After the mixture is eutectic, the sulfur-containing five-membered ring of thioctic acid and sodium thioate will spontaneously open and copolymerize to form a supramolecular polymer. Among them, the random copolymerization between thioctic acid and sodium thioate can effectively quench the sulfur free radical at the end of polythioic acid, and the strong hydrogen bond formed between polythioic acid and sodium polythioate can effectively reduce the potential energy of the system, so the supramolecular polymer formed by deep eutectic can be kept stable at room temperature. Based on the in-situ curing property of the supramolecular polymer and the abundant adhesive carboxyl groups on the polymer skeleton, the supramolecular polymer can achieve stable and high-strength adhesion to a variety of substrates, including wet tissues. Therefore, it can be used as a hot melt adhesive. In addition, the strong hydrogen bonding between sodium polylipoate and polylipoic acid can effectively reduce the dissociation rate of sodium polylipoate in a wet environment, so that the supramolecular polymer adhesive can gradually dissociate and release the biologically active small molecule sodium lipoate when used in a wet environment, thereby playing an anti-inflammatory, bactericidal and antioxidant role, accelerating wound healing. The adhesive was used to replace surgical sutures for rapid sealing of skin wounds to examine its effect of accelerating wound healing, confirming that its effect on promoting the healing of epidermal incisions is better than traditional surgical sutures.

[0012] The preparation method of the present invention is simple, has a wide range of material sources, and is highly practical. The thermal ring-opening polymerization of lipoic acid is actually a deep eutectic phenomenon, which is mainly driven by multiple hydrogen bonds between the carboxyl groups at the ends of the lipoic acid monomers. Therefore, inspired by the deep eutectic mechanism, introducing stronger hydrogen bond interactions in the lipoic acid system may significantly reduce the melting temperature of the system, making it closer to body temperature, and increasing its application in the biomedical field. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a bar graph showing the melting temperature test results of mixtures of lipoic acid and sodium lipoate in different mass ratios in the present invention.

[0014] Figure 2 These are macroscopic pictures of mixtures of lipoic acid and sodium lipoate in different mass ratios before and after heating in the present invention.

[0015] Figure 3 It is the infrared spectra of lipoic acid and sodium lipoate and adhesives of different compositions in the present invention, wherein a is the spectrum and b is a local enlarged view of the infrared spectra of adhesives of different compositions.

[0016] Figure 4The XRD graphs of the lipoic acid monomer and polymers of different compositions in the present invention are shown in Figure 1, wherein a is the XRD graph of the lipoic acid monomer and b is the XRD graph of the adhesives of different compositions.

[0017] Figure 5 It is the Raman spectrum diagram of lipoic acid and sodium lipoate monomers and polymers with different compositions in the present invention.

[0018] Figure 6 It is a bar graph of tensile stress and strain results of adhesives with different compositions in the present invention.

[0019] Figure 7 It is a bar graph showing the test results of the adhesion strength of adhesives of different compositions to different substrates in the present invention.

[0020] Figure 8 It is a bar graph showing the test results of monomer release efficiency of LA-DESP-2 in the present invention.

[0021] Fig. 9 It is a bar graph showing the test results of DPPH removal efficiency of the LA-DESP-2 adhesive of the present invention.

[0022] Fig.10 It is a bar graph showing the test results of the bactericidal efficiency of the LA-DESP-2 adhesive of the present invention against Staphylococcus aureus and Escherichia coli.

[0023] Fig.11 These are photos of the repair effects of skin wounds treated in different ways. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with specific examples. The present invention is further described below in conjunction with examples, but these examples are not intended to limit the present invention.

[0025] Prepare a powder mixture with a mass ratio of 0.5, 1, 1.5, 2, 2.5 and 3 of thioctic acid and sodium thioctic acid respectively, grind it fully and heat it at different temperatures (42-180 degrees Celsius), wait for it to be completely melted, and obtain a hot melt adhesive. In the preparation scheme, the mass of the sodium thioctic acid used remains unchanged, and the mass ratio between thioctic acid and sodium thioctic acid is changed to obtain adhesives of different proportions. The adhesive obtained is named LA-DESP-x, wherein x represents the mass ratio of thioctic acid to sodium thioctic acid. Such as LA-DESP-1.5 (or LA / LA-Na-1.5) is an adhesive obtained by deep eutectic when the mass ratio of thioctic acid and sodium thioctic acid is 1.5. The thioctic acid-based deep eutectic supramolecular polymer adhesive of each component prepared is used for the characterization of material structure, adhesion and the test of basic performance inside and outside the organism. In the present invention, the comprehensive performance of the lipoic acid-based deep eutectic supramolecular polymer adhesive is explained through the thermodynamic properties of the mixture powder and the structure, adhesion performance, biocompatibility and in vivo application effect of the obtained adhesive.

[0026] like Figure 1 As shown in the figure, the thermodynamic properties of mixtures of different compositions of lipoic acid (LA) and sodium lipoate (LA-Na) are shown. From the results, it can be seen that the thermal melting temperature of pure lipoic acid is about 65°C. When the carboxyl group at the end of lipoic acid is deprotonated to obtain sodium lipoate, it cannot show the thermal melting phenomenon even when heated to 200°C, indicating that the multiple hydrogen bonds between the carboxyl groups at the end of lipoic acid are crucial to achieve the thermal melting of the monomer. However, when lipoic acid and sodium lipoate are mixed, the melting temperature of the mixture shows a significant decrease with the increase of the lipoic acid content in the system. When the mass ratio of lipoic acid to sodium lipoate is 0.5, the melting temperature of the mixture is about 180°C. When the mass ratio of lipoic acid is further increased to 2, the melting temperature of the mixture is significantly reduced to about 49°C, showing an obvious deep eutectic phenomenon. When the mass ratio of lipoic acid to sodium lipoate was further increased to 3, the melting temperature of the mixture was further reduced by about 42°C, which was significantly lower than the melting temperatures of pure lipoic acid and sodium lipoate, once again indicating that deep eutectic occurred between the two.

[0027] like Figure 2 As shown, macroscopic images of mixtures of lipoic acid and sodium lipoate powders in different mass ratios after one-step heating and cooling, according to Figure 1In the melting point test, the melting temperature is selected to be higher than the melting point to achieve melting. As can be seen from the picture, although pure lipoic acid can be melted after being heated to its melting point, the melted material will immediately depolymerize after cooling to room temperature and turn into an opaque oligomer. Even if pure polylipoic acid is heated to 200°C, it cannot be melted. However, when the ratio of lipoic acid to sodium lipoate is 0.5, 1, 1.5 and 2, it can remain stable even if it is cooled to room temperature after being heated to melt, indicating that the random copolymerization between sodium lipoate and lipoic acid and the strong hydrogen bond between the two contribute to the stability of polylipoic acid. However, when the content of lipoic acid continues to increase to 2.5 and 3, the polymer formed after it is melted and cooled to room temperature will also depolymerize. This is because when the content of lipoic acid is too much, the sodium lipoate in the system is insufficient to stabilize all polylipoic acid, so polylipoic acid will partially depolymerize.

[0028] like Figure 3 As shown in the figure, this figure is the infrared spectrum of the reaction monomer and the obtained polymer. From the results, it can be seen that compared with the pure lipoic acid monomer, sodium lipoate has a higher -1 The -OH peak at 1700 cm-1 disappeared, and the -C=O peak in the carboxyl group disappeared from 1700 cm-1. -1 Moved to 1545cm -1 , indicating that the carboxyl groups on the sodium lipoic acid structure have been completely deprotonated. As for the prepared adhesive, carboxyl groups and carboxylate structures appear simultaneously in its structure, indicating that polylipoic acid and sodium polylipoic acid exist simultaneously in the adhesive. Figure 3 As shown in a. In the adhesive, the -C=O peak of the carboxylate on the sodium polylipoic acid skeleton has undergone a significant red shift, indicating that the -C=OO - The structure forms a strong hydrogen bond with the -COOH on the polylipoic acid backbone, such as Figure 3 As shown in b.

[0029] like Figure 4 As shown in the figure, the XRD patterns of lipoic acid monomer and polymers with different compositions show that the single lipoic acid monomer is highly crystalline. Figure 4As shown in a, in the structures of LA-DESP-1 and LA-DESP-1.5, the crystallization peaks of lipoic acid monomers all disappeared, indicating that polylipoic acid did not depolymerize in these two polymers. However, a smaller diffraction peak appeared in a smaller diffraction area, indicating that a highly regularly arranged structure appeared in LA-DESP-1 and LA-DESP-1.5, which was caused by the regular arrangement of sodium polylipoic acid in the system. Continuing to increase the content of lipoic acid, the intensity of the diffraction peak gradually decreased to disappear, indicating that the introduction of lipoic acid monomers can destroy the regular arrangement of sodium polylipoic acid and transform it from an ordered crystalline structure to an amorphous structure. Continuing to increase the content of lipoic acid, it was found that the monomer diffraction peak of lipoic acid appeared in LA-DESP-2.5 and LA-DESP-3 polymers, once again illustrating that when the content of lipoic acid is too high, the formed polylipoic acid is unstable in the system and it will undergo further depolymerization, such as Figure 4 As shown in b.

[0030] like Figure 5 As shown in the figure, the Raman spectra of lipoic acid and sodium lipoate monomers and polymers with different compositions. It can be seen from the figure that when the mass ratio of lipoic acid to sodium lipoate is 1 and 2, the lipoic acid in the adhesive obtained is at 511cm -1 The characteristic peak at 493 cm -1 and 515cm -1 There are two peaks at 511cm. This indicates that the sulfur-containing five-membered ring has opened and is stable after opening without depolymerization. When the mass ratio of lipoic acid to sodium lipoate is 3, lipoic acid is at 511cm -1 The peak at did not split but became broadened, indicating that part of the polylipoic acid in the adhesive was depolymerized.

[0031] The mechanical properties test method is to use a cutter to cut the prepared composite adhesive patches of different compositions into dumbbell shapes, perform tensile tests using a tensile machine, and record tensile stress and tensile strain. The tensile speed is 50 mm / min. For detailed tensile process steps, please refer to the literature Chunyan Cui, Tengling Wu, Fei Gao, Chuanchuan Fan, Ziyang Xu, Hongbo Wang, Bo Liu, Wenguang Liu*, An Autolytic High Strength Instant Adhesive Hydrogel for Emergency Self-Rescue, Advanced Functional Materials, 2018, 28, 1804925. Figure 6As shown in the figure, the tensile stress and strain results of adhesives with different compositions. It can be seen from the results that with the increase of lipoic acid content, the tensile stress of the adhesive first decreases and then increases, while the strain, on the contrary, first increases and then decreases. This is because the internal structure of the adhesive changes from crystalline to amorphous and then to crystalline.

[0032] The adhesion strength test method used in this experiment is the lap shear method. The adhesive patch is cut into a square sample of 10mm*10mm in size, one side of it is adhered to the wet pigskin surface, and the other side is adhered with another piece of pigskin. After gently pressing for 10 seconds, the test is immediately carried out. During the test, the two pieces of pigskin are fixed on the tensile machine respectively, and the pigskin is stretched at a certain speed. The stretching speed is 50mm / min. For detailed stretching process steps, please refer to the literature Chunyan Cui, Chuanchuan Fan, Yuanhao Wu, Meng Xiao, Tengling Wu, Dongfei Zhang, Xinyu Chen, Bo Liu, Ziyang Xu, Bo Qu, Wenguang Liu*Water-Triggered Hyperbranched Polymer Universal Adhesives: From Strong Underwater Adhesion to Rapid Sealing Hemostasis, Advanced Materials, 2019, 31, 1905761. Figure 7 As shown in the figure, the adhesion strength of adhesives with different compositions to different substrates. From the results, it can be seen that the adhesion strength of the adhesive to the solid substrate shows a trend of first decreasing and then increasing with the increase of lipoic acid content, which is consistent with the trend of the bulk strength of the adhesive, such as Figure 7 As shown in a-e, the bulk strength of the adhesive is very important in its adhesion performance. Since LA-DESP-2 can remain stable at room temperature and its melting temperature is close to body temperature, LA-DESP-2 was selected as a tissue adhesive to test its adhesion to tissues. The results showed that it can adhere to different tissues, and the highest adhesion strength to pig skin can reach 55kPa. Figure 7 As shown in figure f.

[0033] Weigh different compositions of adhesives in PBS and keep the concentration of the materials in PBS at 10mg / ml. Place the prepared solution in a constant temperature oven at 37°C and measure the ultraviolet absorption at different times. The measurement range of ultraviolet absorption is 200-500nm. And calculate the release amount of different composition materials in artificial saliva at different times through the ultraviolet absorption standard curve of sodium lipoic acid in artificial saliva. The monomer release efficiency is: the monomer release amount at different times / the total amount of monomer in the material. Figure 8 As shown in the figure, the monomer release efficiency of LA-DESP-2. Because sodium polylipoate is water-sensitive, it will spontaneously dissociate into sodium lipoate monomers when it encounters water. Sodium lipoate has excellent antioxidant and antibacterial effects. Therefore, the effective release of sodium lipoate monomers is crucial for the application of adhesives in vivo. The content of sodium lipoate in saliva was measured by soaking the adhesive in artificial saliva for different periods of time. Figure 8 As shown, the sustained release of sodium lipoate can be achieved in the patches of various compositions, and the release efficiency shows a slight decrease with the increase of lipoic acid content, which overcomes the defect of too fast release of single sodium polylipoate.

[0034] Based on the excellent antioxidant capacity of sodium lipoic acid small molecules, it showed a good effect of scavenging free radicals. Fig. 9 As shown, due to the efficient release of small molecules by LA-DESP-2, it showed a very good effect of scavenging DPPH free radicals, which laid the foundation for its application in vivo. The test process can be referred to the published literature Yang Liu, Xiaoping Zhang, Tengling Wu, Bo Liu, Jianhai Yang, Wenguang Liu*, Chinese herb-crosslinked hydrogel bearing rBMSCs-laden polyzwitterion microgels: Self-adaptive manipulation of micromilieu and stemness maintenance for restoring infarcted myocardium, Nano Today, 2021, 41, 101306.

[0035] Based on the excellent antibacterial properties of lipoic acid-based small molecules, we tested the bactericidal effect of LA-DESP-2 against Escherichia coli and Staphylococcus aureus. Fig.10As the bacterial culture time increases, the sodium lipoic acid small molecules in the patch are gradually released and show a bactericidal effect. After 48 hours of co-culture with bacteria, the bactericidal rate can still reach more than 80%. The test process can refer to the published literature Xinyu Bian, Chunyan Cui, Ying Qi, Yage Sun, Zhuodan Zhang, and Wenguang Liu*, Amino Acid Surfactant-Induced Superfast Gelation of Silk Fibroin for Treating Noncompressible Hemorrhage, Advanced Functional Materials, 2022, 32, 2207349.

[0036] Based on the excellent tissue adhesion and life activity of LA-DESP-2, it was developed into a tissue adhesive to replace surgical sutures to accelerate skin wound healing. In the rat back skin injury model, we found that the use of lipoic acid-based adhesives can quickly adhere and seal the wound, accelerate wound healing, and the repair effect is better than traditional surgical sutures. Fig.11 shown.

[0037] According to the content of the present invention, the process parameters can be adjusted to achieve the preparation of the bioadhesive, and the performance shown by the test is basically consistent with the present invention. The above is an exemplary description of the present invention. It should be noted that any simple deformation, modification or other equivalent replacement that can be made by other technicians in this field without spending creative labor falls within the protection scope of the present invention without departing from the core of the present invention.

Claims

1. A lipoic acid-based deep eutectic supramolecular polymer adhesive, characterized in that: After thioctic acid and sodium thioctic acid are mixed and ground, the mixture is heated to melt and then cooled to room temperature. The mass ratio of thioctic acid to sodium thioctic acid is (0.5-3):1, and the melting temperature is 180-42 degrees Celsius.

2. A lipoic acid-based deep eutectic supramolecular polymer adhesive according to claim 1, characterized in that: The mass ratio of lipoic acid to sodium lipoate is (0.5-2):

1.

3. The lipoic acid-based deep eutectic supramolecular polymer bioadhesive according to claim 1, characterized in that: The melting temperature is 49-180 degrees Celsius.

4. A method for preparing a lipoic acid-based deep eutectic supramolecular polymer adhesive, characterized in that: After thioctic acid and sodium thioctic acid are mixed and ground, the mixture is heated to melt and then cooled to room temperature. The mass ratio of thioctic acid to sodium thioctic acid is (0.5-3):1, and the melting temperature is 180-42 degrees Celsius.

5. The method for preparing a lipoic acid-based deep eutectic supramolecular polymer adhesive according to claim 4, characterized in that: The mass ratio of lipoic acid to sodium lipoate is (0.5-2):

1.

6. The method for preparing a lipoic acid-based deep eutectic supramolecular polymer adhesive according to claim 4, characterized in that: The melting temperature is 49-180 degrees Celsius.

7. Use of the lipoic acid-based deep eutectic supramolecular polymer adhesive according to any one of claims 1 to 3 in the preparation of wound adhesion / repair materials.

8. The use according to claim 7, characterized in that: The raw materials of lipoic acid and sodium lipoate and the product of lipoic acid-based deep eutectic supramolecular polymer adhesive are sterilized.

Citation Information

Patent Citations

  • Preparation method of photo-crosslinking dynamic reversible supramolecular polymer adhesive based on lipoic acid small molecular compound

    CN113061263A

  • Preparation method of supramolecular polymer with superstrong adhesion performance in water

    CN113336960A

  • Lipoic acid-based hydrogel as well as preparation method and application thereof

    CN114058014A

  • Lipoic acid hydrogel as well as preparation method and application thereof

    CN115232329A

  • Apparatuses, methods, and compositions for the treatment and prophylaxis of chronic wounds

    US20120245540A1

Cited By

  • Hot-melt injectable adhesive as well as preparation method and application thereof

    CN119823707A