Preparation method of ski core composite material

By using carbon fiber and glass fiber fabric combined with foam interlayer in the ski core, and employing finite element analysis and VARI molding process, the weight, elasticity, and environmental protection issues of the ski core have been solved, achieving the production of high-performance, low-cost skis.

CN118949386AActive Publication Date: 2024-11-15TIANJIN POLYTECHNIC UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411292230.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-15
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Existing ski core materials suffer from problems such as excessive weight, insufficient elasticity, susceptibility to corrosion, and interface delamination. Furthermore, traditional adhesives are prone to environmental pollution, affecting the skiing experience and safety.

Method used

Carbon fiber fabric and glass fiber fabric are used as panel materials, combined with foam sandwich, and the stress conditions are simulated by finite element analysis. Gradient stitch density and angle are designed, and composite materials are prepared using VARI molding process to form a full-thickness stitched foam sandwich structure.

Benefits of technology

This has improved the mechanical properties, durability, and damage tolerance of skis, reduced production costs, and enabled the production of lightweight, high-strength, and environmentally friendly ski cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949386A_ABST
    Figure CN118949386A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a snowboard core composite material. Carbon fiber fabric and glass fiber fabric are selected as panel materials of a snowboard core; sequentially laying a lower-layer carbon-glass fiber panel, a foam interlayer and an upper-layer carbon-glass fiber panel in a layer form to form a prefabricated body; the preparation method comprises the following steps: firstly, preparing a carbon fiber-glass fiber mixed reinforced resin material, then simulating the stress condition of a snowboard by adopting a finite element, performing gradient stitching with different densities and angles on the preform according to the stress to increase the mechanical property, and finally, tightly combining the carbon fiber-glass fiber mixed reinforced resin material with a sandwich material by adopting a VARI process to form a full-thickness stitched foam sandwich structure composite. The carbon fiber and glass fiber mixed reinforced resin composite material is adopted as the shell material, and the puncture stitching technology and the gradient stitching method are combined, so that the mechanical property, the bearing capacity and the damage tolerance of the snowboard core are optimized, the layering of the snowboard core is effectively improved, the durability and the damage tolerance of the snowboard are improved, and the service life of the snowboard is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite materials, in particular to a method for preparing a composite material for a snowboard core. Background Art

[0002] With the advancement of materials science, the ice and snow industry has made great progress. The manufacturing materials of skis have been gradually optimized. Foam sandwich composite materials have been widely used in various fields such as aerospace, shipbuilding, automobiles and sports equipment due to their excellent processability, isotropy, light weight, high strength and simple molding.

[0003] At present, the core of the snowboard is mostly made of wood, which has disadvantages such as being too heavy, insufficient in elasticity and easy to corrode. Compared with wood materials, the snowboard developed with fiber-reinforced resin-based composite materials can improve the quality of the snowboard, have better controllability and vibration reduction performance, and extend its service life. The strength and stability of glass fiber materials allow the snowboard to slide smoothly on different slopes and snow conditions, making glass fiber snowboards one of the mainstream materials for modern snowboards. The use of carbon fiber not only has the effect of lightweighting, but also helps to accurately control the rigidity of the snowboard, providing athletes with a better control experience.

[0004] However, the use of carbon fiber or glass fiber materials alone cannot overcome the defects of the materials themselves, and the combination of carbon fiber and resin is not very tight. All these defects affect the application of these materials and methods in the core of snowboards. The adhesive used in the preparation of composite snowboards contains harmful substances and is easy to volatilize, which is easy to pollute the environment and may also affect the skiing experience and safety. Therefore, improving material quality, reducing board weight, improving board elasticity and durability, and using environmentally friendly adhesives and preparation methods are one of the problems that need to be solved in snowboards.

[0005] Currently, the "sandwich" sandwich structure is the mainstream structure of snowboards, and new composite materials are gradually replacing traditional single materials. Adding a sandwich to the traditional composite panel, the sandwich composite material not only has high specific strength, high specific stiffness, good corrosion resistance and fatigue resistance, but also is lighter than poplar. However, the sandwich composite material is prone to interface delamination, which leads to the destruction of the sandwich composite material, thereby reducing the integrity and durability of the structure. Therefore, it is of great significance to design a composite method for application on the core of the snowboard to prepare a foam sandwich composite material. Summary of the invention

[0006] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a composite material for a snowboard core.

[0007] The technical solution of the present invention to solve the technical problem is to provide a method for preparing a composite material for a snowboard core, characterized in that the method comprises the following steps:

[0008] Step 1, material preparation: select carbon fiber fabric and glass fiber fabric as the panel material of the snowboard core; then cut the carbon fiber fabric, glass fiber fabric and foam interlayer into the corresponding size of the snowboard core;

[0009] Step 2, preparation of a preform: laying a lower carbon-fiberglass panel, a foam interlayer, and an upper carbon-fiberglass panel in layers in sequence to form a preform;

[0010] Step 3: Use finite element analysis software to simulate and analyze the stress of the ski board when a person stands, and obtain a stress cloud map of the ski board; then design the stitching density and stitching angle of the preform in step 2 according to the load distribution in the stress cloud map;

[0011] Step 4, preparation of a fiber composite material reinforcement: according to the stitching density and stitching angle of different stress areas of the preform obtained in step 3, the preform in step 2 is stitched by using a stitching thread through a puncture stitching technique, and the lower carbon-glass fiber panel, the foam interlayer and the upper carbon-glass fiber panel are stitched together to obtain a fiber composite material reinforcement;

[0012] Step 5: Use VARI molding process to solidify and mold the fiber composite reinforcement of step 4 to obtain a snowboard core composite material.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The present invention selects carbon fiber fabric and glass fiber fabric as the panel material of the core of the snowboard; then lays a lower carbon-glass fiber panel, a foam interlayer and an upper carbon-glass fiber panel in layers to form a preform; then uses finite element method to simulate the stress condition of the snowboard, and performs gradient stitching of different densities and angles on the preform according to the stress to increase the mechanical properties; finally, uses a low-cost non-autoclave VARI process to tightly combine the carbon fiber-glass fiber hybrid reinforced resin material with the sandwich material to form a full-thickness stitched foam sandwich structure composite.

[0015] (2) The present invention adopts a resin composite material reinforced by a mixture of carbon fiber and glass fiber as the shell material, and combines puncture suture technology and gradient suture method to optimize the mechanical properties, load-bearing capacity and damage tolerance of the core of the snowboard, effectively improve the core stratification, improve the durability and damage tolerance of the snowboard, and extend its service life.

[0016] (3) The present invention adds a gradient design based on stitching to flexibly improve the stress state of the snowboard core, thereby making the stitching technology play the greatest advantage.

[0017] (4) The present invention prepares the panel material by alternating the carbon fiber fabric and the glass fiber fabric at ±45°, and combines PMI foam as the sandwich material to ensure the elasticity, mechanical properties and lightweight characteristics of the snowboard core.

[0018] (5) The present invention simulates the stress condition of the ski board through finite element method, adjusts the stitching density, realizes gradient distribution, and improves the mechanical properties of the overall ski board.

[0019] (6) The present invention adopts a low-cost and efficient VARI molding process to reduce production costs, improve production efficiency, ensure product quality, and achieve industrialized production, thereby making the snowboard more competitive. The process has no size requirements for the product and is suitable for simple curved surface products such as the snowboard core. The resin is always in a vacuum bag, which can reduce the release of volatiles during the curing process.

[0020] (7) The snowboard core prepared by the present invention has the advantages of light weight, high strength, high performance and low cost, which meets the demand for high-performance snowboards, improves the independent research and development and manufacturing level of the snowboard industry, promotes the development of the snowboard industry, and promotes the development of the entire ice and snow industry chain. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the preform of the present invention;

[0022] Figure 2 Schematic diagram of the distribution of the three-dimensional snowboard model, stress cloud map and stitching density according to Example 1 of the present invention;

[0023] Figure 3 It is a schematic diagram of the structure of the fiber composite material reinforcement of the present invention;

[0024] Figure 4 Graph showing the shear strength and shear modulus test results of Example 1 of the present invention;

[0025] Figure 5 This is a graph showing the bending strength test results of Example 1 of the present invention;

[0026] Figure 6 This is a graph showing the bending modulus test results of Example 1 of the present invention;

[0027] Figure 7 This is a graph showing the bending stiffness test results of Example 1 of the present invention.

[0028] In the figure, there are a lower carbon-fiberglass panel 1, a foam interlayer 2, an upper carbon-fiberglass panel 3, and a stitching line 4. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the claims of the present invention.

[0030] The present invention provides a method for preparing a composite material for a snowboard core (hereinafter referred to as the method), characterized in that the method comprises the following steps:

[0031] Step 1, material preparation: select carbon fiber fabric and glass fiber fabric as the panel material of the snowboard core; then cut the carbon fiber fabric, glass fiber fabric and foam interlayer 2 into the corresponding size of the snowboard core;

[0032] Preferably, in step 1, the carbon fiber fabric is a carbon fiber plain weave fabric; in this embodiment, the specification of the carbon fiber plain weave fabric is 3k and the linear density is 198g / km.

[0033] Preferably, in step 1, the glass fiber fabric is glass fiber plain woven fabric; in this embodiment, the specification of the glass fiber plain woven fabric is 300tex and the linear density is 295g / km.

[0034] Preferably, in step 1, the foam interlayer 2 is made of PMI (polymethacrylimide) foam; PMI foam has light weight, high strength and excellent thermal insulation performance, providing an ideal lightweight and strengthening effect for the board core; the density of PMI foam is 75kg / m 3 .

[0035] Preferably, in step 1, taking an adult as an example, the cutting size is 160 cm×110 cm.

[0036] Step 2, preparation of a preform: laying a lower carbon-glass fiber panel 1, a foam interlayer 2 and an upper carbon-glass fiber panel 3 in layers in sequence to form a preform;

[0037] The lower carbon-glass fiber panel 1 is prepared by laying the carbon fiber fabric in a +45° direction to form a first layer (which contacts the ground when in use) in the form of layers, and then laying the glass fiber fabric in a -45° direction to form a second layer, and then laying the carbon fiber fabric and the glass fiber fabric alternately at intervals until the laying thickness requirement is reached, and the uppermost layer is the glass fiber fabric (which contacts the lower surface of the foam interlayer 2);

[0038] The upper carbon-glass fiber panel 3 is prepared by laying the glass fiber fabric in a +45° direction to form a first layer (which contacts the upper surface of the foam interlayer 2), and then laying the carbon fiber fabric in a -45° direction to form a second layer, and then laying the glass fiber fabric and the carbon fiber fabric alternately at intervals until the laying thickness requirement is reached, and the uppermost layer is the carbon fiber fabric (which contacts the human foot when in use);

[0039] Preferably, in step 2, according to the prescribed standards for skis, the thickness of the lower carbon-glass fiber panel 1 and the upper carbon-glass fiber panel 3 are both 1 mm; in this embodiment, according to the needs and the thickness requirements of the fabric material, the lower carbon-glass fiber panel 1 and the upper carbon-glass fiber panel 3 are both laid with 4 layers, namely two layers of carbon fiber fabric and two layers of glass fiber fabric.

[0040] Preferably, in step 2, the laying angle is ±45°, which allows the fabric to perform optimally. The fabric laid at this laying angle can exhibit optimal mechanical properties and is not easily deformed.

[0041] Step 3: Use finite element analysis software to simulate and analyze the stress of the ski when a person stands, and obtain a stress cloud map of the ski; then design the stitching density and stitching angle of the preform in step 2 according to the load distribution in the stress cloud map to meet the requirements of the composite material for high performance and durability;

[0042] Preferably, step 3 specifically includes:

[0043] S1. Establishing a three-dimensional snowboard model: firstly, according to the geometric shape and size of the snowboard, using drawing software to establish an accurate three-dimensional model of the snowboard, and then obtaining a three-dimensional snowboard model; then importing the three-dimensional snowboard model into the finite element analysis software;

[0044] S2. Material property setting: In the finite element analysis software, specify material properties for the three-dimensional snowboard model;

[0045] Preferably, in step S2, the Young's modulus is set to 850 GPa, the Poisson's ratio is set to 0.22, and the density is set to 2.54 g / cm 3 , these parameters reflect the elasticity and density characteristics of the ski material.

[0046] S3. Analysis step module selection: In the analysis step module of the finite element analysis software, select the analysis type as dynamics, and simulate the force of the ski during the movement through dynamic analysis;

[0047] Preferably, in step S3, the interaction time between the ski board and the ground is set to 5 seconds to simulate a typical skiing process.

[0048] S4. Meshing: Meshing the three-dimensional snowboard model;

[0049] Preferably, in step S4, a three-dimensional solid element (C3D8R) is selected to define the model, and the grid size is set to 0.8 mm.

[0050] Preferably, in step S4, the grid division needs to be fine enough to capture the detailed features of the snowboard, while avoiding too many grids that lead to excessive calculation. In this embodiment, a total of 60,000 grids are divided, which is a result of balancing calculation accuracy and efficiency.

[0051] S5. Boundary condition setting: In order to simulate the connection between the snowboard and the binding, use the binding constraint (Tie) to fix the part where the base plate of the 3D snowboard model is connected to the binding to ensure that the base plate will not be displaced or rotated when the snowboard is subjected to force;

[0052] S6. Apply load: Apply a downward load at the binding position to simulate the force applied by the skier on the skis. The size and direction of the load are adjusted according to the actual situation.

[0053] Preferably, in step S6, the load is 1 kN.

[0054] S7, stress and strain calculation: submit the simulation job in the job module of the finite element analysis software, and the finite element analysis software calculates the three-dimensional snowboard model to obtain stress and strain results;

[0055] S8. Stress cloud map analysis: After the calculation is completed, the stress cloud map is viewed in the visualization module of the finite element analysis software. The stress cloud map displays the stress distribution of each part of the ski board when it is subjected to force in a color-coded manner; by analyzing the stress cloud map, the stress distribution of each part of the ski board when it is subjected to force is obtained;

[0056] S9. Design optimization: Based on the analysis results of the stress cloud map, the stitching density and stitching angle of each stress area of ​​the ski board are optimized to increase the mechanical properties, and the stitching density and stitching angle of each stress area of ​​the ski board are determined, and then the stitching density and stitching angle of the preform corresponding to the design step 2 are determined.

[0057] Preferably, in step S9, in the stress cloud map, the suture density is reduced in the order of red area, orange area, yellow area, green area and blue area, wherein the suture density in the red area is the largest and the suture density in the blue area is the smallest; the amount of suture density reduction between stress areas is determined based on experience.

[0058] Preferably, in step S9, the stitching density is gradually reduced in the order of the red area, the orange area, the yellow area, the green area and the blue area; the gradient reduction is in the form of an arithmetic progression, expressed as: an =a1+(n-1)d, a1 represents the maximum stitching density, and d represents the amount of stitching density reduction. In this embodiment, according to the area and stitching efficiency of the snowboard, the maximum stitching density a1=10mm×10mm, and the stitching density is reduced by a gradient of d=5mm×5mm. According to the gradual decrease in force, the stitching density gradient in other areas is reduced to 15mm×15mm and 20mm×20mm.

[0059] Preferably, in step S9, the strength of the region is increased by increasing the suture density to increase the stress dispersion effect; the suture density is increased in the following ways: (1) increasing the number of sutures in the region to increase the suture density; (2) adjusting the positions of the sutures to arrange the sutures on a path with greater stress to increase the stress resistance.

[0060] Preferably, in step 3 or S9, the stitching angle of the preform is adjusted according to the magnitude and direction of the stress: the stress direction is perpendicular to the surface of the ski board, the stitching angle is parallel to the surface of the ski board, and the stitching line 4 can disperse the stress to the maximum extent.

[0061] Step 4, preparation of a fiber composite material reinforcement: according to the stitching density and stitching angle of different stress areas of the preform obtained in step 3, the preform of step 2 is stitched by using a stitching thread 4 through a puncture stitching technique, and the lower carbon-glass fiber panel 1, the foam interlayer 2 and the upper carbon-glass fiber panel 3 are stitched together to obtain a fiber composite material reinforcement;

[0062] Preferably, in step 4, the puncture suture is different from the traditional suture method. There is no bottom line on the surface of the sutured preform. Single needle suture is used, and there is no knot between the surface sutures, so that both sides of the carbon-glass fiber panel are evenly loaded, which effectively enhances the interlayer performance of the composite material, improves its interlayer bonding strength, reduces the risk of delamination damage, and effectively reduces the impact of friction on the performance of the composite material during the suture process. The puncture suture technology uses a puncture suture device; the puncture suture device uses the shaping mold of the carbon fiber box-type preform disclosed in 201510113258.7. The device is different from the chain suture and lock suture methods, and can sew thick (the thickness is determined by the length of the sewing needle) and hard sewing materials.

[0063] Preferably, in step 4, according to the limited range of the needle pitch and line pitch of the puncture suturing device, the maximum value of the suture density is 1 mm×1 mm.

[0064] Preferably, step 4 is specifically as follows: during suturing, the preform obtained in step 2 is first clamped with a clamp of a puncture and suturing device and fixed on the frame of the puncture and suturing device, and then a hole is drilled on the preform with a puncture head, and then a needle tube is inserted into the drilling position of the preform; then a suture needle with suture thread 4 (a hand-sewing needle is used in this embodiment) is pressed against the needle tube, and while the needle tube is withdrawn, the suture needle with suture thread 4 passes through the preform, and the suture thread 4 moves a distance of a needle pitch under the drive of the suture needle, and then the suture needle is pressed against the needle tube again, the needle tube is withdrawn, and the suture needle passes through the preform along the drilled hole to complete a suturing action; the suturing action is repeated to complete the suturing of the entire preform to obtain a fiber composite material reinforcement.

[0065] Preferably, in step 4, the diameter of the drilling needle is 1.2 mm, the diameter of the suture needle is 1 mm, and the diameter of the drilling needle is slightly larger than the suture needle.

[0066] Preferably, in step 4, the suture thread 4 is made of carbon fiber with light weight, high strength and good toughness; the specification of the carbon fiber is 3k, and double strands are used for suture.

[0067] Step 5: Use VARI (vacuum assisted) molding process to solidify and mold the fiber composite reinforcement of step 4 to obtain a snowboard core composite material.

[0068] Preferably, in step 5, the specific steps of the VARI molding process are as follows:

[0069] A1. Apply a release agent in the snowboard core mold, lay the fiber composite reinforcement of step 4 in the snowboard core mold, lay a release cloth on the fiber composite reinforcement, and place a guide tube at an appropriate position; then put the whole into a vacuum bag and seal it with a sealant;

[0070] A2. Connect the guide tube to the resin tank containing the resin, check the air tightness of the vacuum bag and start the vacuum pump to gradually reduce the pressure in the vacuum bag to promote the resin to penetrate into the fiber composite reinforcement, fill the fiber gaps and infiltrate the fibers; use a flat tool to scrape the resin in the vacuum bag to promote uniform distribution of the resin; maintain the vacuum state for 15 minutes to remove air, and close the vacuum bag after the resin is fully infiltrated;

[0071] Preferably, in step A2, the resin is 6349 epoxy resin, which is obtained by mixing 6439 resin A and 6439 resin B in a mass ratio of 2:1.

[0072] A3. According to the curing characteristics of the resin, put it in an oven and heat it from room temperature to 80°C for 10 minutes. The curing process is maintained for 3 hours. Maintaining a vacuum state helps to discharge volatiles and bubbles in the resin and ensure the quality of the prepared composite material.

[0073] A4. After curing is completed, stop the vacuum pump, take it out after cooling down, trim the burrs with scissors to obtain the snowboard core composite material.

[0074] Example 1

[0075] Step 1, material preparation: select carbon fiber plain weave cloth. In this embodiment, the specification of the carbon fiber plain weave cloth is 3k and the linear density is 198g / km.

[0076] Glass fiber plain woven fabric: in this embodiment, the specification of the glass fiber plain woven fabric is 300tex and the linear density is 295g / km.

[0077] The foam interlayer 2 is made of PMI closed-cell foam, and the density of PMI closed-cell foam is 75kg / m 3 .

[0078] Step 2: Prepare a preform; the layer laying angle is ±45°.

[0079] In this embodiment, according to the demand and the thickness requirement of the fabric material, the lower carbon-glass fiber panel 1 and the upper carbon-glass fiber panel 3 are both laid with 4 layers:

[0080] The preparation of the lower carbon-glass fiber panel 1 is as follows: in the form of layers, the carbon fiber fabric is laid in the direction of +45° to form the first layer (which contacts the ground when in use), and then the glass fiber fabric is laid in the direction of -45° to form the second layer, and then the carbon fiber fabric is laid in the direction of +45° to form the third layer, and then the glass fiber fabric is laid in the direction of -45° to form the fourth layer (which contacts the lower surface of the foam interlayer 2).

[0081] The preparation of the upper carbon-glass fiber panel 3 is as follows: in the form of layers, the glass fiber fabric is laid in the +45° direction to form the first layer (which contacts the upper surface of the foam interlayer 2), and the carbon fiber fabric is laid in the -45° direction to form the second layer, and the glass fiber fabric is laid in the +45° direction to form the third layer; and the carbon fiber fabric is laid in the -45° direction to form the fourth layer (which contacts the human foot when in use).

[0082] In step 3, ABAQUS is used as the finite element analysis software and AutoCAD is used as the drawing software.

[0083] Step 4: preparing a fiber composite reinforcement; Figure 2 As shown, the suture densities are 20mm×20mm, 15mm×15mm, and 10mm×10mm respectively.

[0084] Step 5: Use VARI (vacuum assisted) molding process to solidify and mold the fiber composite reinforcement of step 4 to obtain a snowboard core composite material.

[0085] The experiment tests the properties of the composite material, including horizontal tension, horizontal compression, lateral compression, shear, bending mechanical properties and compression strength after impact. Three specimens with stitching densities of 20mm×20mm, 15mm×15mm and 10mm×10mm were taken from the composite material of the snowboard core.

[0086] Depend on Figure 4 It can be seen that the shear strength of the samples with a stitching density of 20mm×20mm, 15mm×15mm, and 10mm×10mm were increased by 54%, 85%, and 187% respectively compared with the unstitched samples, and the shear modulus was increased by 31.19%, 71.05%, and 117.17% respectively. Therefore, stitching can significantly improve the shear strength and shear modulus of the sample, and with the increase of stitching density, the shear performance of the sample increases accordingly, and the stitching density is positively correlated with the increase in shear strength. The shear strength and shear modulus of the sample with a stitching density of 10mm×10mm are the highest, with the shear strength reaching 2.87MPa and the shear modulus reaching 100.67MPa.

[0087] Under shear load, the foam interlayer 2 in the unstitched sample is subjected to shear stress, and a whole crack appears. The foam bears stress alone, so the shear strength and modulus are correspondingly low. However, the stitched foam interlayer 2 can bear greater stress due to the presence of the suture resin column. The fracture strength of the suture resin column is much higher than that of the foam interlayer 2. Therefore, cracks first appear in the foam interlayer 2 at the suture stress concentration point. As the load increases, the suture resin column begins to break. Therefore, the stitched sample has better shear performance. Among the tested suture densities, the shear performance of the sample improves with the increase of suture density. The suture density of 10mm×10mm has the most significant improvement on the performance of the sample. This is because the denser suture resin column provides better mechanical support and stress distribution, thereby enhancing the overall performance of the sample.

[0088] Depend on Figure 5-Figure 7 It can be seen that the bending strength of the samples with stitching density of 20mm×20mm, 15mm×15mm and 10mm×10mm respectively increased by 11.53%, 26.02% and 38.21% compared with the unstitched samples, the bending stiffness increased by 15.09%, 33.19% and 44.53% respectively, and the bending modulus increased by 15.2%, 33.33% and 38.34% respectively. The bending strength, bending modulus and bending stiffness of the unstitched composite material are much smaller than those of the stitched one. The bending strength, bending modulus and bending stiffness of the composite materials with different stitching density are also different, among which the one with stitching density of 10mm×10mm is the best.

[0089] The stitching density has a great influence on the bending performance of the specimens. The higher the stitching density, the better the bending performance of the specimens. The increase in stitching density significantly enhances the bending performance of the composite material, because more stitches increase the connection points between the panels and the foam sandwich 2, thereby improving the overall stability and load-bearing capacity of the structure. This helps to disperse and transmit the applied bending force, reduce the risk of interlayer separation, and improve energy absorption and dissipation capabilities, while increasing the shear strength of the material. Together, the performance of the composite material under bending loads is improved.

[0090] Therefore, through gradient stitching, the load-bearing capacity and damage tolerance are significantly improved compared to the composite material of the unstitched foam interlayer 2, indicating that the snowboard core composite material of the present invention exhibits higher structural efficiency.

[0091] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A method for preparing a composite material for a snowboard core, characterized in that: The method comprises the following steps: Step 1, material preparation: selecting carbon fiber fabric and glass fiber fabric as the panel material of the snowboard core; then cutting the carbon fiber fabric, glass fiber fabric and foam interlayer (2) into the corresponding size of the snowboard core; Step 2, preparation of a preform: laying a lower carbon-glass fiber panel (1), a foam interlayer (2) and an upper carbon-glass fiber panel (3) in layers in sequence to form a preform; Step 3: Use finite element analysis software to simulate and analyze the stress of the ski board when a person stands, and obtain a stress cloud map of the ski board; then design the stitching density and stitching angle of the preform in step 2 according to the load distribution in the stress cloud map; Step 4, preparation of a fiber composite material reinforcement: according to the stitching density and stitching angle of different stress areas of the preform obtained in step 3, the preform of step 2 is stitched by using a stitching thread (4) through a puncture stitching technique, and the lower carbon-glass fiber panel (1), the foam interlayer (2) and the upper carbon-glass fiber panel (3) are stitched together to obtain a fiber composite material reinforcement; Step 5: Use VARI molding process to solidify and mold the fiber composite reinforcement of step 4 to obtain a snowboard core composite material.

2. The method for preparing the composite material for the core of a snowboard according to claim 1, characterized in that: In step 1, the carbon fiber fabric is carbon fiber plain fabric; the glass fiber fabric is glass fiber plain fabric; and the foam interlayer (2) is PMI foam.

3. The method for preparing the composite material for the core of a snowboard according to claim 1, characterized in that: In step 2, the lower carbon-glass fiber panel (1) is prepared by laying the carbon fiber fabric in a +45° direction to form a first layer, and then laying the glass fiber fabric in a -45° direction to form a second layer, and then laying the carbon fiber fabric and the glass fiber fabric alternately until the laying thickness requirement is reached, and the uppermost layer is the glass fiber fabric; The preparation of the upper carbon-glass fiber panel (3) is as follows: in the form of layers, glass fiber fabric is laid in a +45° direction to form a first layer, and carbon fiber fabric is laid in a -45° direction to form a second layer, and then the glass fiber fabric and carbon fiber fabric are laid alternately at intervals until the laying thickness requirement is reached, and the uppermost layer is the carbon fiber fabric.

4. The method for preparing the composite material for the core of a snowboard according to claim 1, characterized in that: Step 3 specifically is: S1. Establishing a three-dimensional snowboard model: firstly establishing a three-dimensional snowboard model according to the geometric shape and size of the snowboard to obtain a three-dimensional snowboard model; then importing the three-dimensional snowboard model into the finite element analysis software; S2. Material property setting: In the finite element analysis software, specify material properties for the three-dimensional snowboard model; S3. Analysis step module selection: In the analysis step module of the finite element analysis software, select the analysis type as dynamics, and simulate the force of the ski during the movement through dynamic analysis; S4. Meshing: Meshing the three-dimensional snowboard model; S5. Boundary condition setting: In order to simulate the connection between the snowboard and the binding, the binding constraint is used to fix the part where the base plate of the 3D snowboard model is connected to the binding to ensure that the base plate will not be displaced or rotated when the snowboard is subjected to force; S6. Apply load: Apply a downward load at the binding position to simulate the force applied by the skier on the skis. The size and direction of the load are adjusted according to the actual situation. S7, stress and strain calculation: submit the simulation job in the job module of the finite element analysis software, and the finite element analysis software calculates the three-dimensional snowboard model to obtain stress and strain results; S8. Stress cloud map analysis: After the calculation is completed, the stress cloud map is viewed in the visualization module of the finite element analysis software. The stress cloud map displays the stress distribution of each part of the ski board when it is subjected to force in a color-coded manner; by analyzing the stress cloud map, the stress distribution of each part of the ski board when it is subjected to force is obtained; S9. Design optimization: Based on the analysis results of the stress cloud map, the stitching density and stitching angle of each stress area of ​​the ski board are optimized to increase the mechanical properties, and the stitching density and stitching angle of each stress area of ​​the ski board are determined, and then the stitching density and stitching angle of the preform corresponding to the design step 2 are determined.

5. The method for preparing the composite material for the core of a snowboard according to claim 4, characterized in that: In step S2, the Young's modulus is set to 850 GPa, the Poisson's ratio is set to 0.22, and the density is set to 2.54 g / cm 3 ; In step S3, the interaction time between the ski board and the ground is set to 5 seconds to simulate a skiing process; In step S4, a three-dimensional solid unit is selected to define the model, and the mesh size is set to 0.8 mm; a total of 60,000 meshes are divided; In step S6, the load is 1 kN; In step S9, in the stress cloud map, the suture density is reduced in the order of the red area, the orange area, the yellow area, the green area and the blue area; and the amount of reduction in suture density between stress areas is determined based on experience.

6. The method for preparing the composite material for the core of a snowboard according to claim 5, characterized in that: In step S9, the stitching density is gradually reduced in the order of the red area, the orange area, the yellow area, the green area and the blue area; the gradient reduction is in the form of an arithmetic progression, which is expressed as: a n =a1+(n-1)d, a1 represents the maximum stitching density, and d represents the reduction in stitching density.

7. The method for preparing the composite material for the core of a snowboard according to claim 1 or 4, characterized in that: In step 3, the stitching angle of the preform is adjusted according to the magnitude and direction of the stress: the stress direction is perpendicular to the surface of the snowboard, the stitching angle is parallel to the surface of the snowboard, and the stitching line (4) can disperse the stress to the maximum extent.

8. The method for preparing the composite material for the core of a snowboard according to claim 1, characterized in that: Step 4 is specifically as follows: when suturing, firstly clamp the preform obtained in step 2 with a clamp of a puncture and suturing device and fix it on the frame of the puncture and suturing device, then use the puncture head to drill a hole on the preform, and then insert a needle tube at the drilling position of the preform; then, a suture needle with a suture thread (4) is pressed against the needle tube, and the needle tube is withdrawn while the suture needle with a suture thread (4) passes through the preform, and the suture thread (4) moves a distance of a needle pitch under the drive of the suture needle, and then the suture needle is pressed against the needle tube again, the needle tube is withdrawn, and the suture needle passes through the preform along the drilled hole, completing a suturing action; repeating the suturing action to complete the suturing of the entire preform, and obtaining a fiber composite material reinforcement; The suture (4) is made of carbon fiber; the specification of the carbon fiber is 3k, and double strands are used for suture.

9. The method for preparing the composite material for the core of a snowboard according to claim 1, characterized in that: In step 5, the specific steps of the VARI molding process are as follows: A1. Apply a release agent in the snowboard core mold, lay the fiber composite reinforcement of step 4 in the snowboard core mold, lay a release cloth on the fiber composite reinforcement, and place a guide tube at an appropriate position; then put the whole into a vacuum bag and seal it with a sealant; A2. Connect the guide tube to the resin tank containing the resin, check the air tightness of the vacuum bag and start the vacuum pump to gradually reduce the pressure in the vacuum bag to promote the resin to penetrate into the fiber composite reinforcement, fill the fiber gaps and infiltrate the fibers; scrape the resin in the vacuum bag to promote uniform distribution of the resin; maintain the vacuum state for 15 minutes to remove the air, and close the vacuum bag after the resin is fully infiltrated; A3. According to the curing characteristics of the resin, put it in an oven and heat it from room temperature to 80°C in 10 minutes. The curing process is maintained for 3 hours. Maintaining a vacuum state helps to discharge volatiles and bubbles in the resin. A4. After curing is completed, stop the vacuum pump, take it out after cooling, trim the burrs, and obtain the snowboard core composite material.

10. The method for preparing the composite material for the core of a snowboard according to claim 9, characterized in that: In step A2, the resin used is 6349 epoxy resin, which is obtained by mixing 6439 resin A and 6439 resin B in a mass ratio of 2:1.

Citation Information

Patent Citations

  • Foam sandwich extensional organization composite material and method of producing the same

    CN101342807A

  • Sandwich material with PMI foam core material, and preparation method thereof

    CN102848622A

  • Nonmetal anticorrosion daylighting panel and making method thereof

    CN105835479A

  • Interlaminar-toughened laminated composite material and preparation method thereof

    CN105946303A

  • Method for preparing novel super-high density fiber punched felt

    CN106427101A