Synthesis process of high-capacity microporous aluminum salt adsorbent precursor
By using hydrothermal reaction to form a microporous structure in the preparation process of lithium adsorbent, the problems of high cost and low efficiency of existing lithium adsorbents are solved, and lithium ions in high magnesium and low lithium brine are realized. Efficient extraction and good cycle stability, suitable for large-scale production.
Patent Information
- Application Number
- CN202410582580.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-15
AI Technical Summary
The existing preparation process of lithium adsorbents has problems such as high cost, strict equipment requirements, low efficiency, and insufficient adsorption capacity and recycling capacity, especially in the performance of lithium extraction in high magnesium and low lithium brines.
Using a high-capacity microporous aluminum salt adsorbent precursor, the methylamine is dissolved in water and added aluminum and lithium sources, and cetyl trimethyl ammonium bromide and alkaline solution are added. Hydrothermal reaction is carried out to form a microporous aluminum salt adsorbent precursor with a narrow pore size distribution, improving its lithium adsorption and regeneration properties.
It achieves high selectivity and good cycle stability for lithium ions, is suitable for high magnesium-lithium ratio and high sulfate brine, reduces production costs, and is suitable for large-scale industrial production.
Smart Images

Figure BDA0004834512410000101
Abstract
Description
Technical Field
[0001] The invention relates to a synthesis process of a high-capacity microporous aluminum salt adsorbent precursor. Background Art
[0002] In modern industry, the lithium industry occupies an important position and is the foundation for the development of new energy and new materials industries. Lithium products are widely used in metal smelting, glass and ceramics, refrigeration and lubrication, high-energy batteries, aerospace, nuclear fusion power generation and other fields, and their strategic value is increasingly valued by countries around the world. According to the "New Energy Vehicle Industry Development Plan (2021-2035)" and "Global EV Outlook 2019", it is estimated that the global demand for lithium carbonate will be about 861,000 tons in 2025, and the downstream demand for lithium will be divided into four areas: power batteries, 3C consumer batteries, energy storage batteries and traditional industrial applications. Among them, the demand for lithium carbonate for power batteries is about 578,000 tons, the demand for lithium carbonate for 3C consumer batteries is about 67,000 tons, the demand for lithium carbonate for energy storage batteries is about 59,000 tons, and the demand for lithium carbonate in traditional industries is about 157,000 tons.
[0003] At present, the lithium content in salt lake brine is high, the resources are rich, and the production cost is generally lower than the cost of extracting lithium from ore. It has become the main direction for domestic and foreign companies to develop and produce lithium salts. Extracting lithium from salt lake brine has simple process and low cost. According to statistics, the lithium resource reserves of salt lake brine account for about 70% to 80% of the total lithium resources. Therefore, extracting lithium from salt lake brine to produce lithium carbonate will become the main direction of lithium salt production. At present, the main technologies for extracting lithium from salt lake brine used in the world include salting out, precipitation (including carbonate precipitation, aluminate precipitation, hydrated lithium sulfate crystal precipitation, boron magnesium and boron lithium co-precipitation), extraction, calcination leaching, membrane, adsorption, membrane separation, etc. Among them, the most commonly used in Qinghai, my country are adsorption and membrane. The adsorption production process first uses an adsorbent that is selective for lithium to adsorb lithium ions in salt lake brine, and then elutes the lithium ions to separate lithium ions from other ions, which is convenient for subsequent conversion and utilization. The key to this process is the lithium adsorbent, which is required to eliminate the interference of a large number of alkali metal and alkaline earth metal ions coexisting in the brine, selectively adsorb lithium ions in the brine, and have high adsorption capacity and strength. This method is particularly suitable for the separation of lithium in high-magnesium and low-lithium brines (magnesium-lithium ratio is 500:1 or higher), and is also suitable for brines with relatively low lithium content (lithium content is generally below 300 mg / L). It has good selectivity in such brines and has great advantages over other methods. The ion adsorption method has high production efficiency, and the lithium ion content after desorption is more than 3 times that of the raw brine. The biggest advantage of the adsorption exchange method is that it has great advantages in terms of economy and environmental protection, and the process is simple, the recovery rate is high, and the selectivity is good. Aluminum-based adsorbent is the only adsorbent product that has been industrialized. The adsorbent is a layered double hydroxide LiCl·nAl(OH)3·nH2O. The principle of lithium extraction is to use its special internal structure to block alkali metals and alkaline earth metals with larger ion radius during the lithium adsorption process. However, the adsorption capacity and recycling ability of aluminum-based adsorbents are poor. Therefore, how to improve the adsorption capacity and recycling ability is still the focus of current adsorption research.
[0004] The aluminum-based adsorbents commonly used at present often have shortcomings such as low specific surface area, few pores, and low adsorption capacity for lithium ions, which limits their processing capacity.
[0005] The traditional preparation method of lithium adsorbents uses lithium hydroxide and aluminum chloride. However, due to the soaring cost of lithium salt products at this stage, the cost of lithium adsorbent products has also risen accordingly, and the cost of lithium salt accounts for more than 80% of the ton cost. If the lithium salt is not recycled during the preparation process, the production cost will be too high. At the same time, most of the existing synthesis technologies require the use of ultrasonic equipment or proprietary equipment with a high stirring speed, and the preparation process is complicated and inefficient, so it is not suitable for large-scale adoption.
[0006] CN 114618440B discloses a synthesis process of a lithium salt adsorbent precursor, which requires a large amount of pure water reaction, and natural aging and sedimentation for 12 to 48 hours before two-stage washing with water and organic alcohol. The production efficiency is low, the equipment investment is large, and the organic alcohol remaining in the drying process is extremely flammable.
[0007] CN 106076243A discloses a microporous aluminum salt lithium adsorbent and a preparation method thereof, a filler and a method for enriching lithium ions. The method comprises the following steps: adding a lithium hydroxide solution to a soluble aluminum salt solution at a stirring speed of 500 to 800 rpm at a rate of 100 to 300 mL / h, wherein the ratio of the amount of lithium hydroxide to the soluble aluminum salt is 2:1 to 3:1.03 to form a precipitate embedded with soluble lithium, and then removing the soluble lithium to obtain a microporous aluminum salt lithium adsorbent. The method requires a large amount of lithium hydroxide to be added, and special stirring equipment is required to maintain a high stirring speed. The addition speed is slow, the production capacity is low, the production cost is high, and the saturated adsorption capacity of the obtained microporous aluminum salt lithium adsorbent is low.
[0008] CN 109759006A discloses a method for preparing a lithium adsorbent, which comprises grinding a slurry containing Al(OH)3 and LiCl, and spray drying the slurry after ultrasonic microwave heating to obtain a lithium adsorbent. CN105664840B discloses a method for preparing a modified aluminum salt adsorbent, which comprises using silica microspheres as carriers, loading aluminum oxide on the surface of the microspheres, and preparing the slurry by alkali leaching. The above two methods provide new research ideas for the preparation of aluminum-based adsorbents, but both methods have the disadvantages of strict requirements on equipment and operating conditions, or high energy consumption and high production costs. Summary of the invention
[0009] The purpose of the present invention is to overcome the defects of the prior art and to propose a synthesis process of a high-capacity microporous aluminum salt adsorbent precursor. During the synthesis of the precursor, the reaction crystallization system is mild and controllable, the process is relatively simple, and the production cost is low. The obtained product has strong lithium adsorption performance and regeneration performance.
[0010] This adsorbent is particularly suitable for lithium extraction from brine with a high magnesium-to-lithium ratio, high sulfate type, and salt lake brine with a low lithium concentration. It exhibits high adsorption activity for lithium ions, good selectivity for lithium ions and other impurity ions, and good cycle stability, and is easy to achieve large-scale industrial production.
[0011] In order to achieve the above invention objectives, the specific technical solutions adopted by the present invention are:
[0012] A synthesis process of a high-capacity microporous aluminum salt adsorbent precursor comprises the following steps:
[0013] (1) Under stirring (preferably at room temperature), methylamine is dissolved in water, and an aluminum source and a lithium source are added and dissolved in sequence. The aluminum source and the lithium source are prepared according to an Al / Li molar ratio of 2.5 to 4.5:1 to obtain an aluminum-lithium salt mixed aqueous solution. While stirring, hexadecyltrimethylammonium bromide is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0014] In step (1), the amount of methylamine added is 0.1wt% to 0.3wt% of the mass of the aluminum-lithium salt mixed aqueous solution; the mass of water added: the total mass of the aluminum source and the lithium source is 1.1 to 2.3:1, preferably 1.3 to 1.5:1; the Al / Li molar ratio is preferably 3.0 to 3.5:1; the aluminum source is a soluble inorganic aluminum salt, and the aluminum source is preferably at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; the lithium source is a soluble inorganic lithium salt, and the lithium source is preferably at least one of lithium chloride, lithium sulfate, and lithium nitrate; the amount of hexadecyltrimethylammonium bromide added is 0.01wt% to 0.03wt% of the mass of the aluminum-lithium salt mixed aqueous solution.
[0015] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.2 to 2.5:1, placing the alkali solution in a reaction kettle, adding polyethylene glycol (PEG) equivalent to 0.2 wt% to 0.5 wt% of the mass of the aluminum lithium salt intermediate, and stirring uniformly to obtain a dispersed alkali solution.
[0016] In step (2), the alkali solution is an alkali solution of a readily soluble inorganic alkali, preferably at least one of sodium hydroxide and potassium hydroxide solutions, and the alkali solution preferably has a mass concentration of 20wt% to 35wt%.
[0017] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reaction kettle of step (2) to carry out a hydrothermal reaction. After the addition is completed, continue to keep warm and stir for 1.0 to 3.0 hours, and control the end point pH of the reaction to be 6.5 to 8.5. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0018] In step (3), the addition time of the aluminum lithium salt intermediate is 1.0 to 3.0 hours, and the hydrothermal reaction temperature is 70°C to 95°C.
[0019] (4) filtering, washing, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0020] In step (4), the washing is preferably performed with water, more preferably with three or more levels of countercurrent washing, the amount of washing water is 1 to 3 times the mass of the microporous aluminum salt adsorbent precursor wet material slurry, and the washing time is 0.5 to 3.0 hours. The drying temperature is 70 to 95° C. The water content of the obtained microporous aluminum salt adsorbent precursor product is ≤1wt%.
[0021] Furthermore, in step (1), the aluminum source is calculated based on the molar number of aluminum atoms. For example, 1 mole of aluminum nitrate or aluminum chloride is used as 1 mole of aluminum source, and 1 mole of aluminum sulfate is used as 2 moles of aluminum source. The alkali solution in step (2) is calculated based on the molar number of hydroxide, and the lithium source is calculated based on the molar number of lithium ions.
[0022] Furthermore, in step (1), methylamine is used as a colloidal agent, and the long-chain hexadecyltrimethylammonium bromide molecules are embedded in the hydrothermal reaction by the "delamination-intercalation method", so as to obtain the aluminum salt adsorbent precursor Al (OH) 3 layer with an interlayer spacing of 1.7 to 2.1 nm, and the intercalation rate is greatly improved. At the same time, the chelation effect of methylamine on aluminum ions is used to avoid the serious agglomeration of aluminum hydroxide particles, so that in the subsequent hydrothermal reaction, an aluminum salt adsorbent precursor with a large number of pores can be formed, so that the final product can provide more active sites.
[0023] Furthermore, in step (1), hexadecyltrimethylammonium bromide dissociates in water to form a cation C with a hydrophobic group. 19 H 42 N + During the hydrothermal reaction in step (3), the nanorods are attached to the surface of the aluminum hydroxide particles generated by the hydrothermal reaction through electrostatic attraction, and the formation process of the aluminum hydroxide crystals is affected by the steric effect, resulting in a significant reduction in the diameter and length of the nanorods formed by the aluminum hydroxide, thereby optimizing the specific surface area and pore structure of the aluminum hydroxide and promoting it to form an ordered microporous structure.
[0024] Furthermore, in step (1), hexadecyltrimethylammonium bromide is used as a template, and in combination with methylamine, the pore structure of the aluminum salt adsorbent precursor is controlled and optimized to obtain a narrower pore size distribution, thereby reducing the transmission resistance of the liquid and being more conducive to the transmission and adsorption of lithium ions. Under the above ratio, the aluminum hydroxide formed is a microporous Al(OH)3 layer inner octahedron with a narrow pore size distribution and a good pore structure.
[0025] Furthermore, in step (1), methylamine can inhibit the growth of crystals during the hydrothermal process. When the mass ratio of methylamine is too low, the pore size distribution of the aluminum salt adsorbent precursor is not concentrated, and the size of the Al(OH)3 crystal decreases with the increase of the amount of methylamine added. However, when the amount of methylamine added is too high, it will affect its own deprotonation, which is not conducive to coordination with the metal and affects the pore formation of the adsorbent.
[0026] Furthermore, in step (1), the hexadecyltrimethylammonium bromide cation C 19 H 42 N + It is mainly manifested in the role of transporting growth primitives. If the dosage is too low, C 19 H42 N + If the amount is not enough, the transport growth unit function will be weakened, resulting in the synthetic micropores being not densely distributed, the specific surface area being small, and the adsorption effect of lithium ions being unsatisfactory. 19 H 42 N + As the concentration increases, excess template will block the pores of the prepared microporous aluminum hydroxide.
[0027] Furthermore, in step (1), when the amount of lithium source is too large, the octahedral holes in the microporous Al(OH)3 layer have reached saturation, and the excess lithium source will destroy the pore structure of the microporous aluminum hydroxide adsorbent, thereby affecting the adsorption performance. When the amount is too low, the octahedral holes in the adsorbent Al(OH)3 layer have not reached saturation, and the adsorption effect is poor.
[0028] Furthermore, when the amount of the aluminum source in step (1) and the alkali solution in step (2) is increased, the agglomeration of the synthesized aluminum hydroxide will be aggravated, and in the hydrothermal reaction, larger crystal nuclei will be formed, the size of the crystal nuclei will increase, and they will stack each other to form larger pores, thereby reducing the specific surface area of the aluminum hydroxide. When the amount is reduced, the reaction materials are insufficient, which affects the crystal growth and fails to form a sufficient amount of aluminum hydroxide crystals.
[0029] Furthermore, when the amount of water used in steps (1) and (2) is too large, the concentrations of the aluminum lithium salt intermediate aqueous solution and the dispersed alkali solution are too low, which increases the total amount of the solution and causes excessive energy consumption. When the amount of water used is too low, the concentration of the aluminum lithium salt intermediate aqueous solution is too high, which is not conducive to the uniform addition of the subsequent alkali solution, resulting in the agglomeration of aluminum hydroxide crystals, which is not conducive to the hydrothermal reaction, and the pore size of the formed aluminum salt adsorbent precursor is reduced.
[0030] Furthermore, the polyethylene glycol in step (2) is at least one of PEG-200, PEG-400, PEG-600, PEG-800, PEG-1000, PEG-1500, PEG-2000, PEG-3000, PEG-4000, and PEG-6000. PEG is easy to form strong hydrogen bonds with the surface of aluminum salt adsorbent precursor precipitation particles in aqueous solution, and its ether bond is also easy to have affinity with the surface of aluminum salt adsorbent precursor precipitation particles, thereby forming a layer of polymer film, and the serpentine molecular bond makes the protective film have a steric hindrance effect, which greatly weakens the attraction between particles, thereby effectively preventing particle growth and inhibiting the agglomeration of aluminum salt adsorbent precursor particles. In addition, the agglomerates are subsequently opened by grinding in step (4), and these aluminum salt adsorbent precursor primary particles or smaller agglomerates cannot be re-agglomerated into large agglomerates. With the increase of the specific surface area of the particles, the crystals produce a mechanical isolation effect, reducing the average particle size of the particles, so that the agglomeration of the aluminum salt adsorbent precursor powder obtained in this way can be minimized, laying a foundation for the preparation of aluminum salt adsorbent precursors with high adsorption performance. At the same time, it overcomes the limitation of special equipment such as ultrasonic or homogeneous dispersion required by traditional dispersion processes.
[0031] Furthermore, the order of adding materials for the hydrothermal reaction in step (3) is that the aluminum lithium salt intermediate is added to the dispersed alkali solution, the adding time is 1.0 to 3.0 hours, the pH of the reaction is controlled to be 6.5 to 8.5, the microporous aluminum salt adsorbent precursor wet material is LiCl·1.8 to 3.5Al(OH)3·1.0 to 3.9H2O generated by the hydrothermal reaction, and the microporous aluminum salt adsorbent precursor is preferably LiCl·2.0 to 2.3Al(OH)3·1.5 to 2.0H2O. The inventors of the present invention have found through a large number of experimental studies that the use of this reaction condition can ensure that the material can be evenly dispersed in the alkaline system, affect the hydrothermal reaction, and avoid the agglomeration of the aluminum salt adsorbent precursor. At the above-mentioned set temperature, it can not only ensure the uniform dispersion of various particles in the solution, but also avoid the uncontrollable reaction due to the early progress of the hydrothermal reaction. If the temperature is too low, the reaction will not proceed normally; if the temperature is too high, the molecules in the solution will increase their kinetic energy due to the heat, which is not conducive to the formation of stable crystal nuclei. As the number of grains increases, the probability of collision between grains increases, which will cause grain stacking.
[0032] Furthermore, in step (4), the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) is filtered, washed, dried, and ground to obtain a microporous aluminum salt adsorbent precursor product. The washing is preferably performed by water washing, and more preferably by countercurrent washing at least 3 levels. The microporous aluminum salt adsorbent precursor wet material filter cake is dried after three-level countercurrent re-slurry washing. In the three-level countercurrent re-slurry washing, the first-level washing is slurried with the separation mother liquor of the previous second-level washing, the second-level washing is slurried with the separation mother liquor of the previous third-level washing, and the third-level washing is slurried with a certain amount of fresh water. The filter cake is dried and dehydrated to obtain a microporous aluminum salt adsorbent precursor product. The amount of washing water is 1 to 3:1 of the mass of the precursor wet material, and the washing time is 0.5 to 3.0 hours. The filtrate and washing water obtained by filtering the microporous aluminum salt adsorbent precursor wet material slurry can be concentrated and removed from impurities and returned as a lithium salt aqueous solution. The drying temperature of the microporous aluminum salt adsorbent precursor wet material is 70 to 95°C. The water content of the obtained microporous aluminum salt adsorbent precursor product is ≤1wt%.
[0033] The invention discloses a synthesis process of a high-capacity microporous aluminum salt adsorbent precursor. The reaction crystallization system is mild and controllable during the precursor synthesis process, the process is relatively simple, and the production cost is low. The average pore diameter of the obtained product is 1.1-2.0 nm, and the average pore volume is 0.4-0.6 cm 3 / g, and has strong lithium adsorption (lithium adsorption capacity 12-16 mg / g) and regeneration performance. The adsorbent is particularly suitable for lithium extraction from high magnesium-to-lithium ratio, high sulfate brine and low lithium concentration salt lake brine. It shows high adsorption activity, selectivity and good cycle stability for lithium ions and other impurity ions, and is easy to realize large-scale industrial production.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) Hexadecyltrimethylammonium bromide is used as a template, and in the presence of methylamine, the pore structure of the aluminum salt adsorbent precursor is controlled and optimized to obtain a narrower pore size distribution, optimize the specific surface area and pore structure of aluminum hydroxide, and promote the formation of an aluminum salt adsorbent precursor with an octahedral inner Al(OH)3 layer with an ordered microporous structure, so that the final product can provide more active sites and improve the mass transfer efficiency.
[0036] (2) By adding polyethylene glycol (PEG), the crystals are mechanically isolated and the average particle size is reduced. In this way, the agglomeration of the aluminum salt adsorbent precursor powder obtained is minimized, while overcoming the limitation of the traditional dispersion process on special equipment such as ultrasound or homogeneous dispersion.
[0037] (3) The multi-stage countercurrent washing process of the wet material of the microporous aluminum salt adsorbent precursor can, on the one hand, elute the soluble inorganic components in the precursor, and on the other hand, it is all made of water. At the same time, the filtrate and washing water can be concentrated and impurities removed and returned as a lithium salt aqueous solution, which greatly reduces the production cost of the aluminum salt adsorbent.
[0038] (4) The precursor synthesis process can be carried out with the help of existing conventional equipment. The preparation process is simple, the reaction and aging time are short, the production efficiency is higher, the pH of the tail liquid discharged during production is close to neutral, the requirements for equipment and pipeline materials are low, the process is environmentally friendly, and it is more suitable for large-scale production.
[0039] (5) The reaction crystallization system is moderate and controllable during the process. The average pore diameter of the microporous aluminum salt adsorbent precursor product is 1.1-2.0 nm, and the average pore volume is 0.4-0.6 cm 3 / g, and has strong lithium adsorption (lithium adsorption capacity 12 ~ 16mg / g), regeneration performance, and stable structure. The adsorbent is suitable for lithium extraction from high magnesium-lithium ratio, high sulfate brine and low lithium concentration salt lake brine. It shows high adsorption activity for lithium ions, good selectivity for lithium ions and other impurity ions and good cycle stability. The magnesium-lithium ratio can be reduced to below 3:1 through adsorption-desorption, and Li + The desorption rate is greater than 95%. Studies have found that microporous aluminum hydroxide with a pore size between 1.0 and 2.0 nm has better adsorption performance for lithium ions due to its large specific surface area, narrow pore size distribution and a certain order in shape. DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with specific implementation modes.
[0041] Example 1
[0042] The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0043] (1) Under stirring at room temperature, methylamine equivalent to 0.1 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to 1.38 times the total mass of the aluminum source and the lithium source, aluminum chloride hexahydrate and lithium chloride are added in sequence to dissolve, and the aluminum chloride hexahydrate and lithium chloride are prepared according to an Al / Li molar ratio of 3.18:1 to obtain an aluminum-lithium salt mixed aqueous solution. Stirring is maintained, and hexadecyltrimethylammonium bromide equivalent to 0.025 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0044] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.89:1, the alkali solution is a sodium hydroxide solution, and the mass concentration of the sodium hydroxide solution is 25wt%. The alkali solution is placed in a reaction kettle, and polyethylene glycol (PEG-200) equivalent to 0.2wt% of the mass of the aluminum lithium salt intermediate is added, and the mixture is stirred evenly to obtain a dispersed alkali solution.
[0045] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor of step (2) to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 85° C. The aluminum lithium salt intermediate addition time is 2.0 h. After the addition is completed, the stirring is continued for 3.0 h. After the reaction is completed, the end point pH is controlled to be 7.0. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0046] (4) filtering, washing with water, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0047] In step (4), the water washing adopts three-stage countercurrent washing, the washing water volume is 3 times the mass of the microporous aluminum salt adsorbent precursor wet material slurry, and the washing time is 3.0h. The microporous aluminum salt adsorbent precursor wet material filter cake is dried after three-stage countercurrent re-slurry washing. In the three-stage countercurrent re-slurry washing, the first-stage washing uses the separation mother liquor of the previous second-stage washing to make the slurry, the second-stage washing uses the separation mother liquor of the previous third-stage washing to make the slurry, and the third-stage washing uses a certain amount of fresh water to make the slurry. The filtrate and washing water obtained by filtering the microporous aluminum salt adsorbent precursor wet material slurry can be concentrated and removed from impurities and returned for use as a lithium salt aqueous solution.
[0048] The drying temperature is 80° C. The water content of the obtained microporous aluminum salt adsorbent precursor product is 0.26 wt %.
[0049] Example 2
[0050] The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0051] (1) Under stirring at room temperature, methylamine equivalent to 0.20 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to 2.0 times the total mass of the aluminum source and the lithium source, aluminum sulfate and lithium chloride are added in sequence to dissolve, and the aluminum sulfate and lithium chloride are prepared according to an Al / Li molar ratio of 3.5:1 to obtain an aluminum-lithium salt mixed aqueous solution. Stirring is maintained, and hexadecyltrimethylammonium bromide equivalent to 0.03 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0052] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 2:1, the alkali solution is a potassium hydroxide solution, and the mass concentration of the potassium hydroxide solution is 25wt%. The alkali solution is placed in a reaction kettle, and polyethylene glycol (PEG-4000) equivalent to 0.4wt% of the mass of the aluminum lithium salt intermediate is added, and the mixture is stirred evenly to obtain a dispersed alkali solution.
[0053] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor of step (2) to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 90° C. The aluminum lithium salt intermediate addition time is 2.0 h. After the addition is completed, the stirring is continued for 2.0 h. After the reaction is completed, the end point pH is controlled to be 7.5. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0054] (4) filtering, washing with water, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0055] The washing adopts three-stage countercurrent washing, the washing water volume is twice the mass of the microporous aluminum salt adsorbent precursor wet material slurry, and the washing time is 1.0h.
[0056] The drying temperature is 90° C. The water content of the obtained microporous aluminum salt adsorbent precursor product is 0.34 wt %.
[0057] Example 3
[0058] The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0059] (1) Under stirring at room temperature, methylamine equivalent to 0.30 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to 1.3 times the total mass of the aluminum source and the lithium salt, aluminum sulfate and lithium sulfate are added in sequence to dissolve, and the aluminum sulfate and lithium sulfate are prepared according to an Al / Li molar ratio of 2.78:1 to obtain an aluminum-lithium salt mixed aqueous solution. Stirring is maintained, and hexadecyltrimethylammonium bromide equivalent to 0.022 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0060] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 2.0:1, the alkali solution is a potassium hydroxide solution, and the mass concentration of the potassium hydroxide solution is 30wt%. The alkali solution is placed in a reaction kettle, and polyethylene glycol (PEG-400) equivalent to 0.35wt% of the mass of the aluminum lithium salt intermediate is added, and the mixture is stirred evenly to obtain a dispersed alkali solution.
[0061] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor of step (2) to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 70° C. The aluminum lithium salt intermediate addition time is 1.5 h. After the addition is completed, the stirring is continued for 3.0 h. After the reaction is completed, the end point pH is controlled to be 8.0. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0062] (4) filtering, washing, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0063] The amount of washing water is 1 times the mass of the wet slurry of the microporous aluminum salt adsorbent precursor, the washing time is 3.0 h, the drying temperature is 75° C., and the water content of the obtained microporous aluminum salt adsorbent precursor product is 0.42 wt%.
[0064] Example 4
[0065] The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0066] (1) Under stirring at room temperature, 0.15 wt% methylamine equivalent to the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to 1.1 times the total mass of the aluminum source and the lithium salt, aluminum chloride hexahydrate and lithium sulfate are added in sequence to dissolve, and the aluminum chloride hexahydrate and lithium sulfate are prepared according to the Al / Li molar ratio of 3.0:1 to obtain an aluminum-lithium salt mixed aqueous solution. Stirring is maintained, and 0.01 wt% hexadecyltrimethylammonium bromide equivalent to the mass of the aluminum-lithium salt mixed aqueous solution is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0067] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.90:1, the alkali solution is a sodium hydroxide solution, and the mass concentration of the sodium hydroxide solution is 35wt%. The alkali solution is placed in a reaction kettle, and polyethylene glycol (PEG-600) equivalent to 0.25wt% of the mass of the aluminum lithium salt intermediate is added, and the mixture is stirred evenly to obtain a dispersed alkali solution.
[0068] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor of step (2) to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 95° C. The aluminum lithium salt intermediate addition time is 2.5 h. After the addition is completed, the stirring is continued for 2.0 h. After the reaction is completed, the end point pH is controlled to be 7.7. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0069] (4) filtering, washing with water, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0070] The amount of washing water is 1.5 times the mass of the microporous aluminum salt adsorbent precursor wet material slurry, and the washing time is 2.0 hours. The drying temperature is 80° C. The water content of the obtained microporous aluminum salt adsorbent precursor product is 0.12wt%.
[0071] Comparative Example 1
[0072] The synthesis process of the aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0073] (1) Under stirring at room temperature, 0.15 wt% methylamine equivalent to the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to the total mass of the aluminum source and the lithium salt being 1.1:1, aluminum chloride hexahydrate and lithium sulfate are added in sequence to dissolve, and the aluminum chloride hexahydrate and lithium sulfate are in an Al / Li molar ratio of 3.0:1 to obtain an aluminum-lithium salt intermediate.
[0074] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.90:1, the alkali solution is a sodium hydroxide solution, and the mass concentration of the sodium hydroxide solution is 35wt%, and the alkali solution is placed in a reaction kettle to obtain a dispersed alkali solution.
[0075] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor for hydrothermal reaction, the hydrothermal reaction temperature is 95° C., the aluminum lithium salt intermediate addition time is 2.5 h, and after the addition is completed, the stirring is continued for 2.0 h. After the reaction is completed, the end point pH is controlled to be 7.7. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0076] (4) filtering, washing, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0077] The amount of water for washing was 1.5:1 of the mass of the wet precursor, the washing time was 2.0 h, the drying temperature was 80° C., and the microporous aluminum salt adsorbent precursor product with a water content of 0.21 wt% was obtained by grinding.
[0078] Comparative Example 2
[0079] The synthesis process of the aluminum salt adsorbent precursor of this embodiment includes the following steps:
[0080] (1) Under stirring at room temperature, 0.60 wt% methylamine equivalent to the mass of the aluminum-lithium salt mixed aqueous solution is dissolved in water, the amount of water added is equivalent to 1.1 times the total mass of the aluminum source and the lithium salt, aluminum chloride hexahydrate and lithium sulfate are added in sequence to dissolve, and the aluminum chloride hexahydrate and lithium sulfate are prepared according to an Al / Li molar ratio of 3.0:1 to obtain an aluminum-lithium salt mixed aqueous solution. Stirring is maintained, and 0.1 wt% hexadecyltrimethylammonium bromide equivalent to the mass of the aluminum-lithium salt mixed aqueous solution is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate.
[0081] (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.90:1, the alkali solution is a sodium hydroxide solution, and the mass concentration of the sodium hydroxide solution is 35wt%. The alkali solution is placed in a reaction kettle to obtain a dispersed alkali solution.
[0082] (3) Adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reactor for hydrothermal reaction, the hydrothermal reaction temperature is 105° C., the aluminum lithium salt intermediate addition time is 2.5 h, and after the addition is completed, the stirring is continued for 2.0 h. After the reaction is completed, the end point pH is controlled to be 7.7. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained.
[0083] (4) filtering, washing with water, drying and grinding the microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) to obtain a microporous aluminum salt adsorbent precursor product.
[0084] The amount of washing water is 1.5 times the mass of the microporous aluminum salt adsorbent precursor wet material slurry, and the washing time is 2.0 hours. The drying temperature is 80° C. The water content of the obtained microporous aluminum salt adsorbent precursor product is 0.35wt%.
[0085] The above embodiments and comparative examples were tested.
[0086] The microporous aluminum salt adsorbent precursor obtained in each embodiment and comparative example was used as the adsorbent raw material, and an adsorption test was conducted on lithium-containing brine from the Chaerhan chloride-type salt lake in Qinghai, my country. + The content is 245mg / L. + The concentration was determined using an ion chromatograph (THERMO Aquion).
[0087] Adsorption experiment: static adsorption test was adopted, 1000ml of brine was measured and added to a polytetrafluoroethylene beaker, 10g of the microporous aluminum salt adsorbent precursor obtained in the embodiment and the comparative example were taken respectively, and the adsorption and desorption test was carried out by stirring at a speed of 150r / min, the adsorption time was 4h, and the supernatant was taken after adsorption equilibrium, the desorption conditions were 500ml of fresh water desorption, the desorption temperature was 25°C, and the desorption time was 3h. Each group of adsorption and desorption tests was carried out in parallel for 20 groups, and the average value of the sampling and analysis of each ion in 1 / 5 / 10 / 15 / 20 groups was taken as the average adsorption capacity of a single microporous aluminum salt adsorbent precursor, and the adsorption capacity calculation formula was:
[0088] q e =(C0-C e )×V÷m
[0089] Where: q e is the equilibrium adsorption capacity (mg / g); C eis the equilibrium mass concentration of lithium ions (mg / L); C0 is the initial mass concentration of lithium ions (mg / L); V is the volume of the solution (L); m is the dosage of the microporous aluminum salt adsorbent precursor (g). The results are shown in Table 1. The lithium ion adsorption capacity is the equilibrium adsorption capacity, and the pore size and pore volume are the pore size and pore volume of the obtained microporous aluminum salt adsorbent precursor, respectively.
[0090] Table 1
[0091]
[0092] In this specification, unless otherwise specified, all percentages are by mass.
[0093] It can be seen from the above table that in step (2) of comparative example 1, polyethylene glycol was not added, and the pore size, pore volume, lithium ion adsorption capacity and other properties of the obtained product were not as good as those of examples 1-4; while in step (2) of comparative example 2, polyethylene glycol was not added, and the temperature of the hydrothermal reaction was too high, and the pore size, pore volume, adsorption capacity and other properties of the obtained product were worse than those of comparative example 1.
[0094] PEG is easy to form strong hydrogen bonds with the surface of the aluminum salt adsorbent precursor precipitate particles in aqueous solution, and its ether bond is also easy to produce affinity with the surface of the aluminum salt adsorbent precursor precipitate particles, thereby forming a layer of polymer film, and the serpentine molecular bond makes the protective film have a steric hindrance effect, which greatly weakens the attraction between particles, thereby effectively preventing particle growth and inhibiting the agglomeration of aluminum salt adsorbent precursor particles. In addition, the agglomerates are subsequently opened by grinding in step (4), and these aluminum salt adsorbent precursor primary particles or smaller agglomerates cannot be re-agglomerated into large agglomerates. With the increase of the specific surface area of the particles, the crystal grains produce a mechanical isolation effect, reducing the average particle size of the particles, so that the agglomeration of the aluminum salt adsorbent precursor powder obtained can be minimized.
[0095] In Comparative Example 2, the hydrothermal reaction temperature is too high, and the molecules in the solution will increase their molecular kinetic energy due to the heat, which is not conducive to the generation of stable crystal nuclei. As the number of crystal grains increases, the probability of collision between crystal grains increases, which will cause crystal grain stacking.
Claims
1. A synthesis process of a high-capacity microporous aluminum salt adsorbent precursor, characterized in that: The following steps are involved: (1) Under stirring, dissolving methylamine in water, and sequentially adding an aluminum source and a lithium source to dissolve, to obtain an aluminum-lithium salt mixed aqueous solution, while maintaining stirring, adding hexadecyltrimethylammonium bromide to the aluminum-lithium salt mixed aqueous solution, to obtain an aluminum-lithium salt intermediate; (2) preparing alkali solution, placing the alkali solution into a reaction kettle, adding polyethylene glycol, and stirring uniformly to obtain a dispersed alkali solution; (3) adding the aluminum lithium salt intermediate obtained in step (1) to the dispersed alkali solution in the reaction kettle of step (2) to carry out a hydrothermal reaction, and continuing to keep warm and stir after the addition is completed, and controlling the end point pH to 6.5-8.5 after the reaction is completed. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained; (4) The microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) is filtered, washed, dried, and ground to obtain a microporous aluminum salt adsorbent precursor product.
2. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1, characterized in that: The following steps are involved: (1) Under stirring, methylamine is dissolved in water, and an aluminum source and a lithium source are added and dissolved in sequence, wherein the aluminum source and the lithium source are prepared according to an Al / Li molar ratio of 2.5 to 4.5:1 to obtain an aluminum-lithium salt mixed aqueous solution, and while stirring is continued, hexadecyltrimethylammonium bromide is added to the aluminum-lithium salt mixed aqueous solution to obtain an aluminum-lithium salt intermediate; (2) preparing an alkali solution, wherein the molar ratio of the hydroxide in the alkali solution to the aluminum atoms in the aluminum source in step (1) is 1.2 to 2.5:1, placing the alkali solution in a reaction kettle, adding polyethylene glycol equivalent to 0.2 wt% to 0.5 wt% of the mass of the aluminum lithium salt intermediate, and stirring to obtain a dispersed alkali solution; (3) adding the lithium aluminum salt intermediate obtained in step (1) to the dispersed alkali solution in the reaction kettle of step (2) to carry out a hydrothermal reaction, and continuing to keep warm and stir for 1.0 to 3.0 hours after the addition is completed, and controlling the end point pH to 6.5 to 8.5 after the reaction is completed. After the hydrothermal reaction is completed, a microporous aluminum salt adsorbent precursor wet material slurry is obtained; (4) The microporous aluminum salt adsorbent precursor wet material slurry obtained in step (3) is filtered, washed, dried, and ground to obtain a microporous aluminum salt adsorbent precursor product.
3. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: In step (1), the reaction temperature is room temperature; In step (1), the amount of methylamine added is 0.1wt% to 0.3wt% of the mass of the aluminum-lithium salt mixed aqueous solution; the mass of water added: the total mass of the aluminum source and the lithium source is 1.1 to 2.3:1; the Al / Li molar ratio is 3.0 to 3.5:1; the aluminum source is a soluble inorganic aluminum salt; the lithium source is a soluble inorganic lithium salt; and the amount of hexadecyltrimethylammonium bromide added is 0.01wt% to 0.03wt% of the mass of the aluminum-lithium salt mixed aqueous solution.
4. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 3, characterized in that: The aluminum source is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; the lithium source is at least one of lithium chloride, lithium sulfate, and lithium nitrate; the mass of added water: the total mass of the aluminum source and the lithium source is 1.3-1.5:
1.
5. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: In step (2), the alkali solution is a alkali solution of a readily soluble inorganic alkali, and the mass concentration of the alkali solution is 20wt% to 35wt%.
6. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 5, characterized in that: The alkali solution is at least one of sodium hydroxide and potassium hydroxide solution.
7. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: The polyethylene glycol in step (2) is at least one of PEG-200, PEG-400, PEG-600, PEG-800, PEG-1000, PEG-1500, PEG-2000, PEG-3000, PEG-4000, and PEG-6000.
8. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: In step (3), the addition time of the aluminum lithium salt intermediate is 1.0 to 3.0 hours; and the hydrothermal reaction temperature is 70° C. to 95° C.
9. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: In step (4), the washing is performed with water, the amount of washing water is 1 to 3 times the mass of the microporous aluminum salt adsorbent precursor wet material slurry, the washing time is 0.5 to 3.0 hours, and the drying temperature is 70 to 95°C.
10. The synthesis process of the high-capacity microporous aluminum salt adsorbent precursor according to claim 1 or 2, characterized in that: In step (4), water washing adopts three or more levels of countercurrent washing.
Citation Information
Patent Citations
High-capacity zirconium phosphate material for absorbing phenolic compound and preparation method thereof
CN101829544A
Microporous aluminum-salt lithium adsorbent, preparation method therefor, filler and lithium ion enriching method
CN106076243A
Preparation method of Keggin chain structure aluminum lithium adsorbent
CN113926419A
Synthesis process of lithium salt adsorbent precursor
CN114618440A
Mesoporous alumina adsorbent as well as preparation method and application thereof