Solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide as well as preparation method and application of solid acid salt monolithic catalyst

CN118950041APending Publication Date: 2024-11-15SOUTHWEST PETROLEUM UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410969606.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

并且,目前尚未有关于固体酸盐整体式催化剂的报道

Benefits of technology

[0017] (1) Preparation method: Through the preparation method of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide provided by the present invention, M with rich acid and alkali sites, high surface area and excellent oxygen mobility is used. x P y O α -Al 2 O 3 Powder catalyst is used to form a catalyst coating on the surface of cordierite honeycomb ceramic channels through unique coating technology to make high-performance M x P y O α -Al 2 O 3 Monolithic catalyst, this catalyst is suitable for direct synthesis of DMC in a coupled reaction dehydration system in a fixed bed reactor. The metal ion M can be combined with -PO 4 The combination forms a new type of solid acid salt catalyst, which can accurately control the interaction with -PO by changing the metal cation M. 4 The coordination environment, thereby changing the oxygen vacancies and acid-base site concentration of the catalyst, is CO 2 and CH 3 OH activation provides more active sites and effectively couples the reaction dehydration process, forcing the reaction to move forward and improving the reactant conversion rate and target product selectivity in the catalytic reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950041A_ABST
    Figure CN118950041A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of catalysts and particularly relates to a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide as well as a preparation method and application of the solid acid salt monolithic catalyst. The invention relates to a preparation method of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide. The preparation method comprises the following steps: firstly, preparing metal cation salt water and a phosphorus salt water solution, preparing a precipitator solution, mixing the metal cation salt water solution and the phosphorus salt solution for co-precipitation, dropwise adding the water solution into the mixed solution, and adjusting the pH value to obtain a precipitate; the preparation method comprises the following steps: preparing a solid acid salt MxP < 1-x > O < alpha > catalyst, drying and roasting the precipitate obtained in the step S1 to obtain a solid acid salt MxP < 1-x > O < alpha > catalyst, mixing the solid acid salt MxP < 1-x > O < alpha > catalyst, Al2O3 and deionized water, carrying out ball-milling pulping to obtain slurry, soaking a cordierite honeycomb ceramic matrix in the slurry to obtain a cordierite honeycomb ceramic matrix coated with an MxP < 1-x > O < alpha >-Al2O3 composite material, and drying the cordierite honeycomb ceramic matrix coated with the MxP < 1-x > and drying and roasting to obtain the solid acid salt monolithic catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of catalysts, and in particular relates to a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide, a preparation method and an application thereof. Background Art

[0002] Dimethyl carbonate (DMC) is an important chemical raw material and green chemical with a wide range of uses. The price of methanol, its main raw material, will be further reduced with the large-scale industrial production of coal-to-methanol and liquid solar methanol. The direct synthesis of DMC by combining CO2 and CH3OH is of great significance for alleviating the energy crisis and achieving the "dual carbon" goal.

[0003] However, the reaction is restricted by thermodynamic equilibrium limitations and CO2 activation difficulties, the DMC yield is low, and the catalyst is easily poisoned by water, which becomes the key technical bottleneck for its industrial application. Patent CN110882686B discloses a preparation method of a monolithic catalyst for the synthesis of dimethyl carbonate. The Ce-based composite oxide monolithic catalyst used successfully achieves process intensification, and obtains 22% CH3OH conversion rate and 85% DMC selectivity. The reason for this high CH3OH conversion rate is that the monolithic catalyst has the advantage of forcibly removing water during the catalytic process under the non-reactive water removal system, forcing the reaction to proceed in the forward direction. However, the DMC selectivity of this type of monolithic catalyst is mostly around 80%, and how to further improve the activity of the catalyst (reactant conversion rate and product selectivity) has become a technical problem that must be solved before the industrial application of the reaction. Take additional measures to remove water, force the reaction to proceed in the forward direction, and achieve process intensification, which has the great potential to further improve the DMC yield. After years of development, the water removal system has made some progress and is roughly classified into: non-reactive water removal system and reactive water removal system. The non-reactive water removal system is a water removal method that does not participate in the reaction process, usually including: integral catalysts and membrane separation systems, etc., while the reactive water removal system usually uses chemicals such as 2-cyanopyridine and 2,2-dimethoxypropane, which undergo hydrolysis reactions in situ during the reaction process, thereby promoting the reaction to proceed in the forward direction and improving the DMC yield. Under the conditions of the reactor, the in-situ dehydration effect of 2-cyanopyridine as a dehydrating agent was studied, and it was found that CeO2 can promote the in-situ dehydration of the reaction. Some researchers have also tried to combine such dehydrating agents in a gas-solid fixed bed, using CeO2 as a catalyst to obtain a higher methanol conversion rate and DMC selectivity at a lower space velocity, but 2-cyanopyridine causes blockage in the fixed bed reactor under long-term operation, and has a certain deactivation effect on the catalyst. 2,2-Dimethoxypropane (DMP) has become a very potential dehydrating agent, which is green and non-toxic, easy to regenerate, and the dehydration product has no adverse effect on the fixed bed reactor. Through thermodynamic studies, it was found that the addition of DMP can effectively improve the equilibrium constant of the reaction. At present, the research on this dehydrating agent is only carried out in the reactor (not yet applied to the fixed bed reactor), and the conversion efficiency of methanol is relatively low. Therefore, the development of a new catalyst suitable for the DMP reaction dehydration system and its application in the fixed bed reactor is of great significance for promoting the industrial application of the reaction. Coupling the new integral catalyst with the new reaction water removal system and applying it to the fixed bed reactor is a potential implementation path. After years of development, the direct synthesis of DMC catalysts from CO2 and CH3OH can generally be divided into: ionic liquid catalysts, alkaline carbonate catalysts, supported catalysts, and metal oxide catalysts.Ionic liquid catalysts and alkaline carbonate catalysts are homogeneous catalysts. After the reaction, the catalyst, reactants and products are not easy to separate, making it difficult to achieve industrialization; supported catalysts are prone to oxidation deactivation and storage conditions are harsh; while metal oxide catalysts do not have oxidation deactivation, have great advantages in industrial application, and are currently the most widely studied catalysts, mainly based on metal oxides such as cerium. A large number of studies have shown that the acid-base sites on the catalyst surface, especially the acidic centers (Lewis acids and Bronsted acids), are crucial to improving the intrinsic activity of the catalyst. Solid acid salt catalysts have the advantages of good stability, adjustable acidity, and easy product separation, and have the potential to promote the large-scale industrialization of the reaction. In addition, there are currently no reports on solid acid salt monolithic catalysts. At the same time, under a fixed bed reactor, the use of monolithic catalysts coupled with a reaction water removal system (DMP dehydration) has not been reported, so there is an urgent need for a solid acid salt catalyst, preparation method and application for catalytic conversion of carbon dioxide. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for preparing a solid acid salt catalyst for catalytic conversion of carbon dioxide:

[0005] S1: preparing a metal cation salt solution and a phosphate salt aqueous solution in a molar ratio of 1:1 to 9, preparing a precipitant solution, mixing the metal cation salt aqueous solution and the phosphate salt solution for co-precipitation, dropping the precipitant solution into the mixed solution, adjusting the pH, and obtaining a precipitate;

[0006] S2: drying the precipitate obtained in S1 and calcining it to obtain a solid acid salt M x P 1-x O α Catalyst, solid acid salt M x P 1-x O α The catalyst, Al2O3 and deionized water were mixed in a mass ratio of 100:1:1-50, and then ball-milled to obtain a slurry. The cordierite honeycomb ceramic substrate was immersed in the slurry to obtain a honeycomb ceramic substrate coated with M x P 1-x O α -Al2O3 composite cordierite honeycomb ceramic matrix is ​​dried and calcined to obtain a solid acid salt monolithic catalyst.

[0007] Furthermore, the coprecipitation temperature in S1 is 20-90° C., and the pH of S1 is 6-10.

[0008] Furthermore, the drying temperature in S2 is 50-180° C., the drying time is 4-48 hours, and the roasting time is 2-8 hours.

[0009] Furthermore, the calcination temperature in S2 is 400-600°C.

[0010] Furthermore, M described in S2 is any one or any two of Ce, Zr, La, and Ca, the molar ratio of M to P is 9:1 to 1:9, and x is 6 to 8.

[0011] Furthermore, the precipitant described in S1 is any one or any two of urea, ammonium carbonate, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, ammonia water, sodium hydroxide and potassium hydroxide.

[0012] Furthermore, the phosphate salt described in S1 is any one or any two of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, calcium hydrogen phosphate, calcium phosphate, calcium pyrophosphate, potassium dihydrogen phosphate and dipotassium hydrogen phosphate.

[0013] Furthermore, the Al2O3 and M x P 1-x O α The mass ratio of the Al2O3 composite material is 1:100.

[0014] A solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide. The solid acid salt monolithic catalyst is a cordierite honeycomb ceramic structure coated with solid acid salt powder.

[0015] The invention discloses an application of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide. The solid acid salt monolithic catalyst is applied in the preparation of a catalyst.

[0016] Technical Effects

[0017] (1) Preparation method: The present invention provides a method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide, using M having abundant acid and base sites, high surface area and excellent oxygen mobility. x P y O α -Al2O3 powder catalyst, after a unique coating technology, forms a catalyst coating on the surface of the cordierite honeycomb ceramic pores to make high-performance M x P y O α -Al2O3 monolithic catalyst, which is suitable for direct synthesis of DMC in a fixed bed reactor by coupling a reaction dehydration system. Metal ions M can be combined with -PO4 to form a new type of solid acid salt catalyst. By changing the metal cation M, the coordination environment with -PO4 can be accurately regulated, thereby changing the oxygen vacancies and acid-base site concentrations of the catalyst, providing more active sites for CO2 and CH3OH activation, and effectively coupling the reaction dehydration process, forcing the reaction to move forward, and improving the reactant conversion rate and target product selectivity in the catalytic reaction.

[0018] (2) Products: The solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide provided by the present invention uses a monolithic catalyst coupled with a reaction dehydration system for the first time. Compared with general monolithic catalysts or granular catalysts, the reactant conversion rate and the selectivity of the target product are significantly improved. The highest methanol conversion rate is as high as 36.4%, and the selectivity of DMC is as high as 99.6%. This is mainly due to the fact that in the process of the monolithic catalyst timely discharging by-products and water, the catalyst and the dehydrating agent react synergistically, removing water in situ, avoiding poisoning of the catalyst and further promoting the forward reaction, thereby showing excellent catalytic activity, product selectivity and stability.

[0019] (3) Application: The application of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide provided by the present invention has higher economic efficiency in industrial production by simplifying the preparation steps and reducing the production cost. This is of great significance for large-scale production and reducing the overall production cost. The design of the monolithic catalyst coupled reaction dehydration system makes the synergistic effect of the catalyst and the dehydrating agent more efficient, significantly improves the conversion rate of the reactants and the selectivity of the target product, and has significant economic and environmental benefits in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0021] Figure 1 Ce obtained in Example 3 of the present invention 0.8 P 0.2 O α TEM (a) and HRTEM (b) spectra of the powder catalyst.

[0022] Figure 2 is Ce in Example 3 of the present invention 0.8 P 0.2 O α HAADF-STEM (a) and EDS-Mapping (be) spectra of powder catalyst.

[0023] Figure 3 The Ce of Example 3 and Comparative Example 1 of the present invention 0.8 P 0.2 O α -BET spectra of Al2O3 and CeO2-Al2O3 powder catalysts.

[0024] Figure 4 The Ce of Example 3 and Comparative Example 1 of the present invention 0.8 P 0.2 O α -XRD patterns of Al2O3 and CeO2-Al2O3 powder catalysts.

[0025] Figure 5 Ce of Examples 3, 4 and 5 of the present invention 0.8 P 0.2 O α -Al2O3、Zr 0.7 P 0.3 O α -Al2O3、Ca 0.7 La 0.3 O δ -NH3-TPD pattern of Al2O3 catalyst. DETAILED DESCRIPTION

[0026] The following is a combination of Examples 1 to 5 of the present invention, Comparative Examples 1 to 3 and the accompanying Figures 1 to 5 , clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] S1: According to the molar ratio of 6.5:3.5, weigh 10.8321g of La(NO3)2 to prepare a 2.5mol / L La(NO3)2 solution. Weigh 1.54g (NH4)2HPO4 and 3.6mL of ammonia solution (23wt%), transfer the La salt solution and P source precursor to a flask at a constant temperature of 30°C, stir and mix evenly, add ammonia solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0029] S2: The precipitate obtained in S1 was dried at 100°C for 24 hours and calcined at 500°C for 4 hours to obtain solid acid salt La 0.65 P 0.35 O α The obtained block was transferred to a mortar and ground into powder to obtain La 0.65 P 0.35 O α Composite material; solid acid salt La 0.65 P 0.35 O α5 g of the composite material, 0.0501 g of Al2O3 and 3 mL of deionized water were added to a ball mill according to a certain ratio and slurried by ball milling; the cordierite honeycomb ceramic matrix was immersed in the slurry, and the excess slurry was blown off with compressed air, and finally a composite material with La 0.65 P 0.35 O α -Al2O3 composite material coated cordierite honeycomb ceramics, then dried at 100℃ for 12h and calcined at 400℃ in air for 8h to obtain a monolithic catalyst named ZTS-La 0.65 P 0.35 O α -Al2O3, denoted as Cat1.

[0030] Example 2

[0031] S1: According to the molar ratio of 5:5, take 6.9535g of Ce(NO3)2, prepare 2.5mol / L Ce(NO3)2 solution, and weigh 1.8624g (NH4)2HPO4. Take 1.2542g of ammonium carbonate, prepare 23wt%) ammonium carbonate solution, transfer the Ce salt solution and P source precursor to a flask at a constant temperature of 30°C, stir and mix evenly, add ammonium carbonate solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0032] S2: The precipitate obtained in S1 was dried at 100°C for 24h and calcined at 500°C for 4h to obtain solid acid salt Ce 0.5 P 0.5 O α The obtained block was transferred to a mortar and ground into powder to obtain Ce 0.5 P 0.5 O α Composite material; solid acid salt Ce 0.5 P 0.5 O α 5 g of the composite material, 0.0487 g of Al2O3 and 3 mL of deionized water were added to a ball mill according to a certain ratio and slurried by ball milling; the cordierite honeycomb ceramic matrix was immersed in the slurry, and the excess slurry was blown off with compressed air, and finally a composite material with Ce 0.5 P 0.5 O α -Al2O3 composite material coated cordierite honeycomb ceramics, then dried at 100℃ for 12h and calcined at 400℃ in air for 8h to obtain a monolithic catalyst named ZTS-Ce 0.5 P 0.5 O α -Al2O3, denoted as Cat2.

[0033] Example 3

[0034] S1: According to the molar ratio of 8:2, weigh 14.2465g of Ce(NO3)2 to prepare 2.5mol / L Ce(NO3)2 solution. Weigh 0.9145g (NH4)2HPO4 and 5.3mL of ammonia solution (23wt%), transfer the Ce salt solution and P source precursor to a flask at a constant temperature of 30℃, stir and mix evenly, add ammonia solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0035] S2: The precipitate obtained in S1 was dried at 100°C for 24h and calcined at 500°C for 4h to obtain solid acid salt Ce 0.8 P 0.2 O α The obtained block was transferred to a mortar and ground into powder to obtain Ce 0.5 P 0.5 O α Composite material; solid acid salt Ce 0.8 P 0.2 O α 5 g of the composite material, 0.0722 g of Al2O3 and 3 mL of deionized water were added to a ball mill according to a certain ratio and slurried by ball milling; the cordierite honeycomb ceramic matrix was immersed in the slurry, and the excess slurry was blown off with compressed air, and finally a composite material with Ce 0.8 P 0.2 O α -Al2O3 composite material coated cordierite honeycomb ceramics, then dried at 100℃ for 12h and calcined at 400℃ in air for 8h to obtain a monolithic catalyst named ZTS-Ce 0.8 P 0.2 O α -Al2O3, denoted as Cat3.

[0036] Example 4

[0037] S1: According to the molar ratio of 5:5, weigh 7.0495g of Zr(NO3)2 to prepare a 2.5mol / L Zr(NO3)2 solution. Weigh 0.7982g (NH4)2HPO4 and 5.6mL of ammonia solution (23wt%), transfer the Ce salt solution and P source precursor to a flask at a constant temperature of 30°C, stir and mix evenly, add ammonia solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0038] S2: The precipitate obtained in S1 was dried at 100°C for 24 hours and calcined at 500°C for 4 hours to obtain solid acid salt Zr 0.7 P 0.3 O αThe obtained block was transferred to a mortar and ground into powder to obtain Zr 0.7 P 0.3 O α Composite material; Solid acid salt Zr 0.7 P 0.3 O α 5 g of the composite material was mixed with 0.0307 g of Al2O3 and 3 mL of deionized water in a certain proportion and added into a ball mill to prepare a slurry; the cordierite honeycomb ceramic matrix was immersed in the slurry, and the excess slurry was blown off with compressed air to obtain a composite material with Zr 0.7 P 0.3 O α -Al2O3 composite material coated cordierite honeycomb ceramics, then dried at 100℃ for 12h and calcined at 400℃ in air for 8h to obtain a monolithic catalyst named ZTS-Zr 0.7 P 0.3 O α -Al2O3, recorded as Cat4.

[0039] Example 5

[0040] S1: According to the molar ratio of 7:3, weigh 4.9735g of Ca(NO3)2, prepare 2.5mol / L Ca(NO3)2 solution, and weigh 0.4363g (NH4)2HPO4. Take 0.5674g of ammonium carbonate, prepare 23wt% urea solution, transfer the Ca salt solution and P source precursor to a flask at a constant temperature of 30°C, stir and mix evenly, add ammonium carbonate solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0041] S2: The precipitate obtained in S1 was dried at 100°C for 24 hours and calcined at 500°C for 4 hours to obtain solid acid salt Ca 0.7 P 0.3 O α The obtained block was transferred to a mortar and ground into powder to obtain Ca 0.7 P 0.3 O α Composite material; solid acid salt Ca 0.7 P 0.3 O α 5 g of the composite material was mixed with 0.0292 g of Al2O3 and 3 mL of deionized water in a certain proportion and added into a ball mill to prepare a slurry; the cordierite honeycomb ceramic matrix was immersed in the slurry, and the excess slurry was blown off with compressed air to obtain a composite material having Ca 0.7 P 0.3 O α-Al2O3 composite material coated cordierite honeycomb ceramics, then dried at 100℃ for 12h and calcined at 400℃ in air for 8h to obtain a monolithic catalyst named ZTS-Ca 0.7 P 0.3 O α -Al2O3, denoted as Cat5.

[0042] Comparative Example 1

[0043] S1: Weigh 10.3454g of Ce(NO3)2 and prepare a 2.5mol / L Ce(NO3)2 solution. Measure 4.5mL of ammonia solution (23wt%), transfer the Ce salt solution to a flask at a constant temperature of 30℃, stir and mix evenly, add ammonia solution dropwise under vigorous stirring to control the solution pH to 7-8, react for 4h, and obtain a precipitate;

[0044] S2: The precipitate obtained in S1 was dried at 100°C for 24h and calcined at 500°C for 4h to obtain pure CeO2-Al2O3. The obtained block was transferred to a mortar and ground into powder to obtain a pure CeO2-Al2O3 composite material; 5g of the pure CeO2-Al2O3 composite material was added to a ball mill according to a certain proportion with 0.0303g of Al2O3 and 3mL of deionized water, and slurried by ball milling; the cordierite honeycomb ceramic substrate was immersed in the slurry, and the excess slurry was blown off with compressed air to finally obtain a cordierite honeycomb ceramic with a pure CeO2-Al2O3 composite material coating, which was then dried at 100°C for 12h and calcined at 400°C in air for 8h to obtain an integral catalyst, named ZTS-pure CeO2-Al2O3 composite material, denoted as Cat6.

[0045] First, an activity test was conducted by directly synthesizing DMC from CH3OH and CO2 in a fixed bed reactor. The monolithic catalysts prepared in Examples 1 to 5 and Comparative Example 1 were respectively placed in a steel tube reactor at a temperature of 140°C, a pressure of 2.4 MPa, and a space velocity of 2880 h -1 Under the conditions of CO2 to CH3OH feed ratio of 20 and CH3OH to DMP ratio of 10, the composition of the product was analyzed and detected online using Agilent GC7890B gas chromatograph. The test results are shown in Table 1. CH3OH is the methanol conversion rate, S DMC is the selectivity for dimethyl carbonate, Y DMC is the yield of dimethyl carbonate.

[0046] Table 1 Catalyst activity test data

[0047] catalyst <![CDATA[C CH3OH (%)]]> <![CDATA[S DMC (%)]]> <![CDATA[Y DMC (%)]]> Example 1 (Cat 1) 22.3 89.1 19.8 Example 2 (Cat 2) 21.2 97.3 20.6 Example 3 (Cat 3) 36.4 99.6 36.2 Embodiment 4 (Cat 4) 30.4 98.9 29.7 Example 5 (Cat 5) 16.1 73.1 11.8 Comparative Example 1 (Cat 6) 22.3 96.9 21.6

[0048] Then, the conditions with and without the dehydrating agent were compared, and Example 1, Example 3, and Comparative Example 1 were tested. The test process was similar to the activity test, except that the dehydrating agent DMP was not added during the test process. The specific test results are shown in Table 2.

[0049] Table 2 Catalyst activity test data without dehydrating agent

[0050] catalyst <![CDATA[C CH3OH (%)]]> <![CDATA[S DMC (%)]]> <![CDATA[Y DMC (%)]]> Example 1 (Cat 1) 6.3 84.1 5.3 Example 3 (Cat 3) 22.5 86.1 19.4 Comparative Example 1 (Cat 6) 6.5 91.1 5.9

[0051] Comparing Table 1 and Table 2, the integral catalyst coupled reaction dehydration system used in the present invention can greatly improve the conversion rate of methanol. In Cat3, the integral catalyst coupled reaction dehydration system increased the methanol conversion rate of the catalyst from 22.5% to 36.4%. In Cat1, the integral catalyst coupled reaction dehydration system increased the methanol conversion rate of the catalyst from 6.3% to 22.3%. This shows that the integral catalyst coupled reaction dehydration system reported for the first time in the present invention can effectively promote the reaction, and this is due to the fact that the integral catalyst has uniformly coated active particles in contact with the reactants, and water is removed in time to promote the reaction. Secondly, the coupled reaction dehydration strategy, the catalyst and the dehydrating agent react synergistically to remove water in situ, avoid water enrichment, and force the reaction to proceed in the forward direction.

[0052] Combination Figure 1 , showing the best activity of Ce 0.8 P 0.2 O α -TEM and HRTEM spectra of Al2O3 catalyst. The spectra show that the catalyst prepared by the present invention is spherical nanoparticles of uniform size (d = 10.2 ± 1.3nm). At the same time, lattice fringes of 0.312nm belonging to the CeO2 (111) crystal plane and lattice fringes of 0.305nm belonging to the CePO4 (200) crystal plane were found, indicating that the catalyst prepared by the present invention has eight-coordinated and nine-coordinated Ce structures, which is conducive to the generation of unsaturated sites and promotes the activation of reactants.

[0053] Combination Figure 2 It can be seen that Ce, O, and P elements are highly dispersed on the catalyst, indicating that the catalyst of the present invention has a rich CeO2-CePO4 interface structure and produces abundant unsaturated sites. Figure 3 , showing Ce 0.8 P 0.2 O α -Al2O3 catalyst and CeO2-Al2O3 catalyst, Ce 0.8 P 0.2 O α -Al2O3 catalyst exhibits a large specific surface area (95m 2 / g), which is much larger than CeO2-Al2O3 catalyst (46m 2 / g), which is beneficial to provide more activation sites for the reaction molecules and promote the reaction.

[0054] Combination Figure 4 It can be seen that Ce is found in the present invention 0.8 P 0.2 O α -Al2O3 catalyst contains both CeO2 cubic fluorite structure and CePO4 monazite phase. 0.8 P 0.2 O α -The diffraction pattern intensity of Al2O3 decreases sharply, which again indicates that there is a very strong interfacial interaction between CePO4 and CeO2, which can produce more acidic sites, effectively activate the reactants and promote the synergistic dehydration process. Figure 5 The solid acid salt catalyst synthesized by the present invention has weak acid and medium acid, and the appearance of medium acid is often accompanied by the generation of "P-OH" active center, so Ce 0.8 P 0.2 O α -Al2O3、Zr 0.7 P 0.3 O α -Al2O3 is much more active than Ca 0.7 P 0.3 O α -Al2O3 catalyst.

[0055] The present invention provides a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide. The catalyst has abundant acid and base sites and a high surface area, which helps to improve its catalytic activity, and excellent oxygen fluidity helps to improve the stability and efficiency of the catalyst during the reaction. A catalyst coating is formed on the surface of the cordierite honeycomb ceramic pores through a unique coating technology, which enhances the adhesion and durability of the catalyst. The catalyst has a high conversion rate, with the highest methanol conversion rate reaching 36.4%, which indicates that the catalyst can effectively convert reactants into target products during the reaction. The catalyst also has high selectivity, with a DMC selectivity of up to 99.6%, which indicates that the catalyst can catalyze the generation of target products with high specificity and reduce the generation of by-products.

[0056] The present invention provides a method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide. The method adopts room temperature coprecipitation. Catalyst powder is prepared by a simple room temperature coprecipitation method. This method is simple to operate, easy to control, and suitable for large-scale production. The catalyst powder is coated on the surface of the cordierite honeycomb ceramic pores to form a uniform and stable catalyst coating. It is not only easy to scale up production, but also the preparation process is simple and easy to operate, which makes the industrial production of the catalyst feasible and low-cost. The simplified preparation process helps to reduce the production cost of the catalyst, thereby making it more competitive in industrial applications.

[0057] The application of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide provided by the present invention can be suitable for directly synthesizing DMC in a coupled reaction dehydration system in a fixed bed reactor, has high catalytic activity for synthesizing DMC from CO2 and CH3OH, and has high selectivity for DMC; can produce DMC continuously with high yield; and has significant economic and environmental benefits in industrial applications.

Claims

1. A method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide, characterized in that: The following steps are involved: S1: preparing a metal cation salt solution and a phosphate salt aqueous solution in a molar ratio of 1:1 to 9, preparing a precipitant solution, mixing the metal cation salt aqueous solution and the phosphate salt solution for co-precipitation, dropping the precipitant solution into the mixed solution, adjusting the pH, and obtaining a precipitate; S2: drying the precipitate obtained in S1 and calcining it to obtain a solid acid salt M x P 1-x O α Catalyst, solid acid salt M x P 1-x O α The catalyst, Al2O3 and deionized water were mixed in a mass ratio of 100:1:1-50, and then ball-milled to obtain a slurry. The cordierite honeycomb ceramic substrate was immersed in the slurry to obtain a honeycomb ceramic substrate coated with M x P 1-x O α -Al2O3 composite cordierite honeycomb ceramic matrix is ​​dried and calcined to obtain a solid acid salt monolithic catalyst.

2. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The temperature of the coprecipitation in S1 is 20-90°C, and the pH of S1 is 6-10.

3. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The drying temperature in S2 is 50-180°C, the drying time is 4-48h, and the roasting time is 2-8h.

4. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The calcination temperature in S2 is 400-600°C.

5. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The M described in S2 is any one or any two of Ce, Zr, La, and Ca, the molar ratio of M to P is 9:1 to 1:9, and x is 6 to 8.

6. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The precipitant described in S1 is any one or any two of urea, ammonium carbonate, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, ammonia water, sodium hydroxide and potassium hydroxide.

7. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: The phosphate salt described in S1 is any one or any two of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, calcium hydrogen phosphate, calcium phosphate, calcium pyrophosphate, potassium dihydrogen phosphate and dipotassium hydrogen phosphate.

8. The method for preparing a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 1, characterized in that: Al2O3 and M described in S2 x P 1-x O α The mass ratio of the Al2O3 composite material is 1:

100.

9. A solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The solid acid salt monolithic catalyst is a cordierite honeycomb ceramic structure coated with solid acid salt powder.

10. The use of a solid acid salt monolithic catalyst for catalytic conversion of carbon dioxide according to claim 9, characterized in that: The solid acid salt monolithic catalyst is used in preparing a catalyst.

Citation Information

Patent Citations

  • Monolithic catalyst for preparation of dimethyl carbonate by direct synthesis process, preparation method and direct synthesis method of dimethyl carbonate

    CN110882686A

  • Cerium-based composite oxide coating type monolithic catalyst, preparation method and application method thereof

    CN110882687A

  • Catalyst for synthesizing dimethyl carbonate and its application

    CN1380140A

  • Process for making dimethyl carbonate

    US20150141690A1