Ligand-modified heterogeneous catalyst, preparation method thereof and application of ligand-modified heterogeneous catalyst in catalyzing selective hydrogenation reaction of alkyne compounds

The ligand-modified heterophasic catalyst prepared by in-situ regeneration method of phosphine ligands solves the selectivity and stability problems in the semi-hydrogenation of alkynes, achieves high activity and selective catalysis, and is environmentally friendly, suitable for alkynes Selective hydrogenation reaction of compounds-like compounds.

CN118950100APending Publication Date: 2024-11-15ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202410878368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing supported palladium catalysts have selectivity and stability problems in alkyne semi-hydrogenation reaction, especially in high conversion rates, and the palladium utilization rate of traditional Lindlar catalysts is low and environmentally contaminated, making the preparation process cumbersome. , metal particles are prone to agglomeration and active components are prone to loss.

Method used

The ligand-modified heterophasic catalyst is prepared by in-situ reduction method of phosphine ligand. By loading precious metal particles on metal oxides or molecular sieve support, and using triphenylphosphine or tricyclohexylphosphine as ligands, preventing noble metal agglomeration and optimizing reactions Microenvironment, improving catalytic activity and selectivity.

Benefits of technology

High activity and selective catalysis are achieved in both air and hydrothermal stability, the catalyst is stable to air and water, and the selectivity of styrene in the phenylacetylene hydrogenation reaction reaches 98%, and there is no need to introduce lead or quinoline, which is environmentally friendly. The preparation process is simple and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950100A_ABST
    Figure CN118950100A_ABST
Patent Text Reader

Abstract

The invention discloses a ligand-modified heterogeneous catalyst and a preparation method and application thereof in catalyzing selective hydrogenation reaction of alkyne compounds, the catalyst comprises a carrier, noble metal particles loaded on the carrier and phosphine ligands coordinated on the surface of the carrier, the carrier is selected from metal oxides or molecular sieves, the metal oxide carrier is selected from TiO2, Al2O3, ZrO2, ZnO, CeO2 or SiO2, and the phosphine ligands are selected from metal oxides or molecular sieves. The molecular sieve is selected from ZSM-5, SBA-15 or MCM-41, the noble metal is selected from Pd, Rh or Ru, the phosphine ligand is selected from triphenylphosphine or tricyclohexylphosphine, and the loading capacity of noble metal particles on the catalyst is 0.5-5%. The noble metal in the catalyst is reduced on the carrier in situ through triphenylphosphine, agglomeration is prevented under space obstruction of the ligand, and more active sites are provided. The introduction of PPh3 changes the hydrogen cracking mode, and H2 activation is converted from homogeneous cracking to heterogeneous cracking. In addition, PPh3 can also optimize the reaction microenvironment, reduce autopoisoning of alkyne and promote olefin desorption, thereby improving the catalytic activity and selectivity of selective hydrogenation of alkyne compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ligand-modified multiphase catalyst and a preparation method thereof and application of the catalyst in catalyzing the selective hydrogenation reaction of acetylene compounds. Background Art

[0002] Supported palladium catalysts are the preferred catalysts for the semi-hydrogenation of alkynes and are essential in the synthesis of various fine chemicals, pharmaceuticals, and agricultural chemicals. However, due to the presence of a large amount of active hydrogen on the continuous palladium surface, the selectivity for olefins is difficult to exceed 95% when the conversion rate is greater than 99%. In general, the overhydrogenation phenomenon is very serious at high conversion rates. Due to the proportional relationship between the adsorption energies of the various adsorbed components, there is a balance between the activity and selectivity of this reaction.

[0003] Lindlar catalysts, consisting of palladium nanoparticles (NPs) and a calcium carbonate support modified with lead and / or quinoline, have been used for the semi-hydrogenation of alkynes since the 1950s. However, there are some disadvantages of Lindlar catalysts, including the improvement of selectivity at the expense of catalytic activity, low utilization of palladium, and easy reconstruction of the catalyst surface, thus the catalyst stability is not ideal. In addition, the loss of lead during use not only reduces the cyclic stability of the catalyst but also causes environmental pollution. These limitations have stimulated extensive research, and therefore, it is crucial to develop a highly active, selective and environmentally friendly catalyst for the semi-hydrogenation of alkynes.

[0004] Metal oxides and molecular sieves have long attracted great attention in both laboratory research and industrial applications due to their low price and wide availability. 0.5 / Ni 0.5@γ-Al2O3 inherits the high activity of Pd and the high selectivity of Ni. By utilizing the synergistic effect of Pd and Ni, efficient semi-hydrogenation of phenylacetylene was achieved at low temperature and low pressure (ACS Catal. 2022, 12, 24, 14846–14855). Qin's group prepared the ZIF-8 / Pt / SiO2 catalyst by combining atomic layer deposition (ALD) and gas phase conversion. The ZIF-8 film induced an increase in the electron density of the Pt component, which increased the selectivity of olefins in the hydrogenation reaction of 1-heptyne from 14% to 70% (J Fuel Chem Technol. 2021; 49(9): 1316-1325). The subnano PdCx species and reduced silanol in the PdCx@S-1 catalyst promote H2 activation and styrene desorption by forming Si-OC structures, and the rate-determining step changes from styrene hydrogenation to styrene desorption, thereby significantly improving the selectivity of olefins in the selective alkyne hydrogenation reaction (Angew. Chem. Int. Ed. 2023, e202313101). However, this type of heterogeneous catalyst with metal oxides or molecular sieves as carriers still has its inherent shortcomings, such as cumbersome preparation process, easy agglomeration of metal particles, easy loss of active components, etc., which limit the application of this type of heterogeneous catalyst.

[0005] Therefore, it is urgent to develop a green, cheap, simple, efficient and highly stable supported metal catalyst. Due to the uniqueness of the phosphine ligand in-situ reduction method, that is, no additional reducing agent is required, and there is ligand modification on the catalyst surface, the present invention adopts the phosphine ligand in-situ reduction method to prepare the Pd-based heterogeneous catalyst. Summary of the invention

[0006] In view of the above-mentioned technical problems existing in the prior art, the object of the present invention is to provide a ligand-modified multiphase catalyst and a preparation method thereof and application in catalyzing the selective hydrogenation reaction of acetylenic compounds. A multiphase catalyst containing precious metal particles is synthesized by an in-situ ligand reduction method. The multiphase catalyst is stable to air and hydrothermal conditions. It is applied to the selective hydrogenation reaction of acetylenic compounds and exhibits excellent catalytic activity and selectivity.

[0007] The technical solution adopted by the present invention is as follows:

[0008] A ligand-modified multiphase catalyst comprises a carrier, noble metal particles loaded on the carrier and phosphine ligands coordinated on the surface of the carrier, wherein the carrier is selected from metal oxides or molecular sieves, the metal oxide carrier is selected from TiO2, Al2O3, ZrO2, ZnO, CeO2 or SiO2, the molecular sieve is selected from ZSM-5, SBA-15 or MCM-41, the noble metal is selected from Pd, Rh or Ru, preferably Pd; the phosphine ligand is selected from triphenylphosphine or tricyclohexylphosphine, preferably triphenylphosphine; the loading content of the noble metal particles on the catalyst is 0.5-5%.

[0009] Furthermore, the preparation method of the catalyst includes the following steps: putting the carrier into toluene at a solid-liquid ratio of 1g:50-150mL, fully stirring at room temperature, and then adding a calculated amount of a noble metal precursor solution; after fully stirring for 0.5-3h, adding a triphenylphosphine solution dissolved in toluene, stirring in an oil bath at 60-100°C for 5-10h, filtering, washing, and drying to obtain the catalyst.

[0010] The noble metal in the catalyst of the present invention is in-situ reduced on the carrier by triphenylphosphine, and agglomeration is prevented under the spatial barrier of the ligand to provide more active sites. The introduction of PPh3 changes the hydrogen cracking mode, and converts H2 activation from homogeneous cracking to heterogeneous cracking. In addition, PPh3 can also optimize the reaction microenvironment, reduce the self-poisoning of alkynes, promote olefin desorption, and thus improve the catalytic activity and selectivity of the selective hydrogenation of acetylenic compounds.

[0011] Furthermore, the noble metal precursor is Pd(O2CCH3)2, Rh(O2CCH3)3 or Ru(O2CCH3)3; the mass ratio of the noble metal precursor to the carrier is 1:20 to 500, preferably 1:100 to 200.

[0012] Furthermore, the molar ratio of the noble metal precursor to the phosphine ligand is 1:1-10, preferably 1:8-10.

[0013] The present invention also provides an application of the ligand-modified multiphase catalyst in the reaction of catalyzing the selective hydrogenation of acetylenic compounds to prepare corresponding olefinic compounds, wherein the acetylenic compounds are mixed with a solvent, and the mixed reaction liquid is subjected to a hydrogenation reaction with hydrogen under the action of the catalyst to generate olefinic compounds; wherein the reaction temperature is 0 to 100° C., and the reaction pressure is 0.1 to 4 MPa; and the solvent is water, ethanol, dichloromethane, tetrahydrofuran, ethyl acetate, dioxane, dimethyl sulfoxide, n-hexane or toluene.

[0014] Furthermore, the solvent is water or ethanol, preferably ethanol, and the dispersion concentration of the alkyne compound in the solvent is 0.04-0.1 g / mL.

[0015] Furthermore, the mass of the catalyst is 0.1-10%, preferably 1-5%, of the mass of the acetylene compound.

[0016] Furthermore, the temperature for the selective hydrogenation reaction is 20-30° C., the hydrogen pressure is 0.1-0.5 MPa, and the reaction time is 15-60 min.

[0017] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0018] 1. The present invention prepares a heterogeneous catalyst by adding triphenylphosphine (PPh3) or tricyclohexylphosphine to load precious metals on a common metal oxide or molecular sieve carrier. Conventional methods for loading metals include ultrasonic method, deposition-precipitation method, sol-gel method, etc. The present invention preferably uses a simple and efficient ligand in-situ reduction method. The catalyst metal precursor is in-situ reduced on the carrier under the action of PPh3 or tricyclohexylphosphine, and a large number of ligands exist on the carrier and metal surface. The preparation method of the catalyst is simple, short in time, low in production cost, and the product structure is easy to adjust.

[0019] 2. Since the spatial barrier effect of the ligand inhibits the aggregation of precious metals, the catalyst metal particles prepared by the present invention are uniform in size and have good dispersibility. The average diameter of the metal particles can reach 1 to 10 nm. The operation is simple and the reaction conditions are mild. The heterogeneous catalyst is stable to air, water and heat. After being in the air for 6 months, its catalytic activity for hydrogenation of phenylacetylene does not decrease and the metal valence remains unchanged.

[0020] 3. Compared with the traditional commercial Lindlar catalyst, the multiphase catalyst prepared by the present invention does not need to introduce lead or quinoline, and is environmentally friendly. The introduction of PPh3 or tricyclohexylphosphine can change the hydrogen cracking mode, and convert H2 activation from homogeneous cracking to heterogeneous cracking. In addition, PPh3 or tricyclohexylphosphine can also optimize the reaction microenvironment, reduce alkyne self-poisoning, promote the desorption of olefins, and thus improve the catalytic activity and selectivity of the selective hydrogenation of acetylenic compounds. When the catalyst of the present invention is used to catalyze the hydrogenation reaction of phenylacetylene to prepare styrene, the selectivity of styrene reaches 98%, and the conversion rate of phenylacetylene is 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a high-resolution transmission electron microscopy image of the catalyst prepared in Example 1;

[0022] Figure 2 This is a spherical aberration corrected transmission electron micrograph of the catalyst prepared in Example 1. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0024] Example 1 Heterogeneous catalyst based on TiO2 loaded with Pd reduced by triphenylphosphine

[0025] 100 mg TiO2 was placed in a 50 ml round bottom flask, 10 ml toluene was added, and the mixture was stirred at room temperature for 0.5 h, followed by the addition of a calculated amount of 4.6 mmol Pd(O2CCH3)2. After further stirring for 1 h, 5 ml of a PPh3 solution (molar ratio of Pd:PPh3=1:8) dissolved in toluene was added, and the mixture was stirred in an oil bath at 80°C for 8 h. The catalyst Pd / TiO2-PPh3 was obtained by suction filtration, washing, and drying.

[0026] The catalyst prepared in Example 1 was characterized by high resolution transmission electron microscopy (HRTEM) and spherical aberration corrected transmission electron microscopy (AC-TEM). The results are as follows: Figure 1 and Figure 2 As shown. Figure 1 It can be seen that no obvious Pd particles are observed on the catalyst surface. Figure 2 It can be seen that the lattice spacing of the metal particles is 0.227nm, which belongs to the Pd (111) plane. It is confirmed that the catalyst is composed of TiO2 carrier and Pd particles. The Pd particles are highly dispersed on the carrier and have close contact with the TiO2 carrier, indicating that there is an obvious interaction between the metal and the carrier. The average particle size of the Pd particles on the catalyst is about 2 to 4nm.

[0027] The catalysts prepared in Example 1 were characterized by scanning transmission electron microscopy (SEM), and elemental analysis by SEM showed that the Pd content in the catalyst of Example 1 was 0.5%.

[0028] Example 2 Heterogeneous catalyst based on TiO2 loaded with Pd reduced by tricyclohexylphosphine

[0029] The steps for preparing the catalyst were repeated as in Example 1, except that PPh3 was replaced by tricyclohexylphosphine (molar ratio of Pd:tricyclohexylphosphine=1:8), and finally the catalyst Pd / TiO2-tricyclohexylphosphine was obtained.

[0030] Example 3 Heterogeneous Catalyst Based on TiO2 Loaded Rh

[0031] The preparation steps of the catalyst are repeated in Example 1, except that "Pd(O2CCH3)2 is replaced by an equal molar amount of Rh(O2CCH3)3, so that the molar ratio of Rh:PPh3=1:8", and finally the catalyst Rh / TiO2-PPh3 is prepared.

[0032] Example 4 Heterogeneous Catalyst Based on TiO2 Loaded Ru

[0033] The steps for preparing the catalyst are repeated in Example 1, except that "Pd(O2CCH3)2 is replaced by an equal molar amount of Ru(O2CCH3)3, so that the molar ratio of Ru:PPh3=1:8", and finally the catalyst Ru / TiO2-PPh3 is prepared.

[0034] Example 5 Heterogeneous Catalyst Based on Al2O3 Loaded Pd

[0035] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg of Al2O3, and finally the catalyst Pd / Al2O3-PPh3 was prepared.

[0036] Example 6 Heterogeneous Catalyst Based on ZrO2 Loaded Pd

[0037] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg ZrO2, and finally the catalyst Pd / ZrO2-PPh3 was prepared.

[0038] Example 7 Heterogeneous Catalyst Based on ZnO Supported Pd

[0039] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg ZnO, and finally the catalyst Pd / ZnO-PPh3 was prepared.

[0040] Example 8 Heterogeneous Catalyst Based on CeO2 Loaded Pd

[0041] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg CeO2, and finally the catalyst Pd / CeO2-PPh3 was prepared.

[0042] Example 9 Heterogeneous Catalyst Based on SiO2-Loaded Pd

[0043] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg SiO2, and finally the catalyst Pd / SiO2-PPh3 was prepared.

[0044] Example 10 Heterogeneous catalyst based on ZSM-5 loaded with Pd

[0045] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg ZSM-5, and finally the catalyst Pd / ZSM-5-PPh3 was prepared.

[0046] Example 11 Heterogeneous catalyst based on MCM-41 loaded with Pd

[0047] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg MCM-41, and finally the catalyst Pd / MCM-41-PPh3 was prepared.

[0048] Example 12 Heterogeneous Catalyst Based on SBA-15 Loaded Pd

[0049] The steps for preparing the catalyst were repeated as in Example 1, except that the catalyst carrier was replaced with 100 mg SBA-15, and finally the catalyst Pd / SBA-15-PPh3 was prepared.

[0050] Example 13 Preparation of styrene by hydrogenation of phenylacetylene using the heterogeneous catalyst prepared in Example 1

[0051] After 220uL of phenylacetylene, 10mg of the heterogeneous catalyst prepared in Example 1 and 5mL of ethanol were added to a 50mL stainless steel autoclave, the stainless steel autoclave was filled and exhausted with hydrogen 3 times (i.e., the air in the stainless steel autoclave was replaced by hydrogen, and the air in the stainless steel autoclave was emptied, and the following embodiments are equivalent), hydrogen was filled to 0.1MPa and sealed, heated in a 30°C water bath, magnetically stirred, and selective hydrogenation reaction was carried out for 15min. After stopping the reaction, the residual hydrogen in the stainless steel autoclave was carefully discharged and the reaction solution was taken out. The heterogeneous catalyst and the reaction solution were separated by a centrifugal method, and the reaction solution was detected by gas chromatography. The conversion rate of phenylacetylene obtained by detection and calculation was 100%, and the selectivity of styrene was 98%.

[0052] Example 14 Preparation of Styrene by Hydrogenation of Phenylacetylene Using Heterogeneous Catalysts Prepared in Different Examples

[0053] The catalytic experimental steps were repeated in Example 13, except that the catalyst in Example 1 was replaced with a catalyst of equal mass prepared in other examples, and other conditions remained unchanged. The final experimental results are shown in Table 1.

[0054] Table 1

[0055]

[0056]

[0057] The following conclusions can be seen from Example 13 and Table 1:

[0058] 1) By comparing the experimental results of the catalysts of Example 1 and Example 2, it is shown that triphenylphosphine has good reducibility, and its unique structure promotes the reaction and realizes efficient hydrogenation of phenylacetylene.

[0059] 2) Comparison of the experimental results of the catalysts of Examples 1 and 3-4 shows that Pd has the best catalytic activity when selected as the metal precursor, Rh has good activity but low selectivity, and Ru has poor activity.

[0060] 3) By comparing the experimental results of the catalysts in Examples 1 and 5-12, it is shown that the ligand modification method provided by the present invention has good applicability to metal oxide supports or molecular sieve supports, and exhibits excellent performance in the semi-hydrogenation reaction of alkynes.

[0061] The catalysts of Examples 1, 5, and 10 were subjected to repeated application experiments on the recovered multiphase catalysts according to the method of Example 13. The results showed that all three catalysts had good stability: they were not deactivated after 10 applications, and the yield of styrene was maintained above 75%. The Pd content and valence state of the catalysts after application were basically unchanged through ICP, XPS, and TEM detection, and the particle morphology was basically unchanged.

[0062] Embodiment 15

[0063] The catalyst was prepared according to the method of Example 1, except that the amount of "Pd(O2CCH3)2" was adjusted so that the Pd content in the catalyst was changed to 1%, 2%, 3% and 5% respectively through elemental analysis by SEM.

[0064] Example 15 Catalysts containing 1%, 2%, 3% and 5% Pd were reacted according to the method of Example 13, except that the catalyst of Example 1 was replaced with the same mass, and other conditions remained unchanged. The final experimental results were:

[0065] 1) When the catalyst carrier is TiO2 and the content of Pd is 1%, the conversion rate of phenylacetylene is 100% within 17 minutes, and the selectivity of styrene is 96%;

[0066] 2) When the catalyst carrier is TiO2 and the content of Pd is 2%, the conversion rate of phenylacetylene is 100% within 11 minutes, and the selectivity of styrene is 97%;

[0067] 3) When the catalyst carrier is TiO2 and contains 3% Pd, the conversion rate of phenylacetylene is 100% within 7 minutes, and the selectivity of styrene is 96%;

[0068] 4) When the catalyst carrier is TiO2 and the content of Pd is 5%, the conversion rate of phenylacetylene is 100% within 4 minutes, and the selectivity of styrene is 93%.

[0069] Embodiment 16:

[0070] The preparation steps of the catalyst in Example 16 are repeated in Example 1, the only difference being "changing the amount of PPh3 so that the molar ratio of Pd:PPh3=1:1, 1:5 or 1:10", and finally obtaining the catalyst Pd / TiO2-PPh3.

[0071] Example 16 The catalysts prepared under the conditions of molar ratio Pd:PPh3=1:1, 1:5 or 1:10 were reacted according to the method of Example 13, except that the catalyst of Example 1 was replaced with the same mass, and other conditions remained unchanged. The final experimental results were:

[0072] 1) When the catalyst prepared under the condition of molar ratio Pd:PPh3=1:1 was used for catalysis, the conversion rate of phenylacetylene was 63% within 15 minutes, and the selectivity of styrene was 99%;

[0073] 2) When the catalyst prepared under the condition of molar ratio Pd:PPh3=1:5 was used for catalysis, the conversion rate of phenylacetylene was 79% within 15 minutes, and the selectivity of styrene was 96%;

[0074] 3) When the catalyst prepared under the condition of molar ratio Pd:PPh3=1:10 was used for catalysis, the conversion rate of phenylacetylene was 100% within 15 minutes, and the selectivity of styrene was 97%.

[0075] Example 17 The catalyst prepared in Example 1 was placed in air for 6 months to catalyze the hydrogenation of phenylacetylene to produce styrene

[0076] 220uL of phenylacetylene, 10mg of the heterogeneous catalyst prepared in Example 1 (after the catalyst was placed in a cool air environment for 6 months) and 5mL of ethanol were added to a 50mL stainless steel autoclave, and the stainless steel autoclave was filled with hydrogen and exhausted 3 times, and then filled with hydrogen to 0.1MPa and sealed, heated in a 30°C water bath, magnetically stirred, and selective hydrogenation was carried out for 15min. After stopping the reaction, the residual hydrogen in the stainless steel autoclave was carefully discharged, and the reaction solution was taken out. The heterogeneous catalyst and the reaction solution were separated by centrifugation, and the reaction solution was detected by gas chromatography. The detection and calculation showed that the conversion rate of phenylacetylene was 100%, and the selectivity of styrene was 98%.

[0077] Example 18 The catalyst prepared in Example 5 was placed in air for 6 months to catalyze the hydrogenation of phenylacetylene to produce styrene

[0078] 220uL of phenylacetylene, 10mg of the heterogeneous catalyst prepared in Example 5 (after the catalyst was placed in a cool air environment for 6 months) and 5mL of ethanol were added to a 50mL stainless steel autoclave, and the stainless steel autoclave was filled with hydrogen and exhausted 3 times, and then filled with hydrogen to 0.1MPa and sealed, heated in a 30°C water bath, magnetically stirred, and selective hydrogenation was carried out for 15min. After stopping the reaction, the residual hydrogen in the stainless steel autoclave was carefully discharged, and the reaction solution was taken out. The heterogeneous catalyst and the reaction solution were separated by centrifugation, and the reaction solution was detected by gas chromatography. The detection and calculation showed that the conversion rate of phenylacetylene was 12%, and the selectivity of styrene was 98%.

[0079] It can be seen that the catalysts obtained in Examples 1 and 5 have good stability, are inert to air and moisture, and the ligands are stably present and do not leak.

[0080] Embodiments 19 to 37:

[0081] Examples 19 to 37 are examples of preparing functionalized compounds by catalyzing the hydrogenation reaction of various acetylene compounds using the multiphase catalyst prepared in Example 1. The operating steps of Examples 19 to 37 are the same as those of Example 13, except that certain reaction conditions (such as the type of reaction solvent, the type of reaction substrate, and the reaction time) are changed. The specific changed reaction conditions and corresponding reaction effects of each example are shown in Table 1.

[0082] Table 1

[0083]

[0084]

[0085]

[0086] As can be seen from Examples 19-37, when ethanol is used as a solvent, the catalyst can achieve optimal catalytic activity. The catalyst has good universality, and different substituents can be well retained during the reaction, and the alkynyl group can be selectively converted into a double bond. Except for phenylacetylene, no matter whether it is an acetylenic compound containing an electron-donating substituent or an electron-withdrawing substituent, under the action of a catalyst, it can be efficiently converted into a corresponding olefin compound. In addition, for phenylacetylene substituted with halogen (F, Cl, Br, I), the halogen can also be well retained. This is very important in industry, because if the halogen is taken off, the hydrogen halide can greatly corrode the equipment, thereby limiting its application in industry. Simultaneously, no matter for terminal alkynes or intramolecular alkynyl groups, the catalyst has very high catalytic performance.

[0087] Comparative Example 1 Preparation of Styrene Based on Titanium Dioxide Supported Pd Heterogeneous Catalyst

[0088] Catalyst preparation: 100 mg TiO2 was placed in a 50 ml round-bottom flask, 5-15 ml deionized water was added, and the mixture was stirred for 1 hour at room temperature, and then a calculated amount of Pd(O2CCH3)2 solution was added. After further stirring for 1 hour, a NaBH4 solution dissolved in deionized water was added. After stirring for 1 hour, the mixture was filtered, washed, and dried to obtain the catalyst Pd / TiO2-NaBH4.

[0089] Catalytic reaction process: 220uL of phenylacetylene, 10mg of the above-mentioned heterogeneous catalyst and 5mL of ethanol were added to a 50mL stainless steel autoclave. The stainless steel autoclave was filled and exhausted with hydrogen three times, and then filled with hydrogen to 0.1MPa and sealed. It was heated in a water bath at 30°C and stirred magnetically for selective hydrogenation reaction for 15min. After stopping the reaction, the residual hydrogen in the stainless steel autoclave was carefully discharged and the reaction liquid was taken out. The heterogeneous catalyst and the reaction liquid were separated by centrifugation, and the reaction liquid was detected by gas chromatography. The detection and calculation showed that the conversion rate of phenylacetylene was 63% and the selectivity of styrene was 91%.

[0090] Comparative Example 2 Preparation of Styrene Based on Heterogeneous Catalyst Supported by Activated Carbon

[0091] Catalyst preparation: 100 mg of activated carbon (400 mesh) was placed in a 50 ml round-bottom flask, 5-15 ml of toluene was added, and the mixture was stirred at room temperature for 0.5 h, and then a calculated amount of Pd(O2CCH3)2 solution was added. After further stirring for 1 h, a PPh3 solution (molar ratio of Pd:PPh3=1:8) dissolved in toluene was added, and the mixture was stirred in an oil bath at 60-100°C for 5-10 h. The catalyst Pd / C-PPh3 was obtained by suction filtration, washing, and drying.

[0092] Catalytic reaction process: 220uL of phenylacetylene, 10mg of the above-mentioned heterogeneous catalyst and 5mL of ethanol were added to a 50mL stainless steel autoclave. The stainless steel autoclave was filled and exhausted with hydrogen for 3 times, and then filled with hydrogen to 0.1MPa and sealed. It was heated in a water bath at 30°C and stirred magnetically for selective hydrogenation reaction for 15min. After stopping the reaction, the residual hydrogen in the stainless steel autoclave was carefully discharged and the reaction liquid was taken out. The heterogeneous catalyst and the reaction liquid were separated by centrifugation, and the reaction liquid was detected by gas chromatography. The detection and calculation showed that the conversion rate of phenylacetylene was 56% and the selectivity of styrene was 96%.

[0093] It can be seen from Comparative Examples 1 and 2 that the addition of triphenylphosphine ligand can improve the catalyst activity, and the activity of metal oxides and molecular sieves as carriers is better than that of commercial activated carbon.

[0094] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.

Claims

1. A ligand-modified heterogeneous catalyst, characterized in that The catalyst comprises a carrier, precious metal particles loaded on the carrier and a phosphine ligand coordinated on the surface of the carrier, wherein the carrier is selected from metal oxides or molecular sieves, the metal oxide carrier is selected from TiO2, Al2O3, ZrO2, ZnO, CeO2 or SiO2, the molecular sieve is selected from ZSM-5, SBA-15 or MCM-41, the precious metal is selected from Pd, Rh or Ru, preferably Pd; the phosphine ligand is selected from triphenylphosphine or tricyclohexylphosphine, preferably triphenylphosphine; the loading content of the precious metal particles on the catalyst is 0.5-5%.

2. The method for preparing a ligand-modified heterogeneous catalyst according to claim 1, characterized in that The following steps are involved: The carrier is put into toluene at a solid-liquid ratio of 1 g: 50-150 mL, fully stirred at room temperature, and then a calculated amount of a noble metal precursor solution is added; after fully stirring for 0.5-3 hours, a triphenylphosphine solution dissolved in toluene is added, and stirred in an oil bath at 60-100° C. for 5-10 hours. The catalyst is obtained by filtering, washing, and drying.

3. The method for preparing a ligand-modified heterogeneous catalyst according to claim 2, characterized in that The noble metal precursor is Pd(O2CCH3)2, Rh(O2CCH3)3 or Ru(O2CCH3)3; the mass ratio of the noble metal precursor to the carrier is 1:20-500, preferably 1:100-200.

4. The method for preparing a ligand-modified heterogeneous catalyst according to claim 2, characterized in that The molar ratio of the noble metal precursor to the phosphine ligand is 1:1-10, preferably 1:8-10.

5. Use of a ligand-modified heterogeneous catalyst as claimed in claim 1 in catalyzing the selective hydrogenation of acetylenic compounds to prepare corresponding olefinic compounds.

6. The use according to claim 5, characterized in that Alkyne compounds are mixed with a solvent, and the mixed reaction liquid is subjected to a hydrogenation reaction with hydrogen under the action of a catalyst to generate olefin compounds; wherein the reaction temperature is 0-100°C and the reaction pressure is 0.1-4MPa; the solvent is water, ethanol, dichloromethane, tetrahydrofuran, ethyl acetate, dioxane, dimethyl sulfoxide, n-hexane or toluene.

7. The use according to claim 6, characterized in that The solvent is water or ethanol, preferably ethanol, and the dispersion concentration of the alkyne compound in the solvent is 0.04-0.1 g / mL.

8. The use according to claim 6, characterized in that The mass of the catalyst is 0.1-10% of the mass of the acetylene compound, preferably 1-5%.

9. The use according to claim 6, characterized in that The temperature for the selective hydrogenation reaction is 20-30°C, the hydrogen pressure is 0.1-0.5 MPa, and the reaction time is 15-60 min.

Citation Information

Patent Citations

  • Catalyst modified by phosphine ligand, and preparation method and application thereof

    CN111905831A

  • Ultra-dispersed noble metal heterogeneous catalyst and application thereof

    CN111992206A

  • Catalyst for preparing various of organic aldehyde by alefin hydro-formylation and preparation method thereof

    CN1422695A

Cited By

  • Preparation of ligand-modified palladium carbon catalyst and application of ligand-modified palladium carbon catalyst in selective hydrogenation reaction of mifepristone

    CN119733566A

  • Alkylphosphine-guided nanosheet P-coated ZSM-5 molecular sieve as well as preparation method and application thereof

    CN120646857A