Film removing method of FTO glass, perovskite cell and preparation method of perovskite cell
The fluorine-doped tin dioxide film layer on the FTO glass is removed through the reaction of zinc plate and hydrochloric acid, which solves the problem of laser welding failure, realizes the inorganic packaging and water-gas barrier of perovskite batteries, and improves the stability and application level of the battery .
Patent Information
- Application Number
- CN202411315041.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
During the packaging process of perovskite batteries, the fluorine-doped tin dioxide film layer on the surface of the FTO glass is difficult to remove, resulting in laser welding failure, affecting the stability and packaging quality of the perovskite batteries.
The FTO glass is removed by zinc plate and hydrochloric acid. The fluorine-doped tin dioxide film layer is removed through the reaction of SnO2+Zn+4HCl=SnCl2+ZnCl2+2H2O to achieve film removal of the FTO glass. Laser welding packaging can be carried out later.
The fluorine-doped tin dioxide film layer on the FTO glass was successfully removed, and the optical transmittance and reflectivity of the glass was maintained, and the inorganic packaging of perovskite batteries was realized, almost completely blocking water and gas, improving perovskite The stability of the battery and the level of industrial application.
Smart Images

Figure CN118954972A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of packaging technology, and in particular to a method for removing a film from FTO glass, a perovskite cell and a method for preparing the same. Background Art
[0003] As an emerging photovoltaic technology, perovskite cells have the advantages of relatively low material and production costs, high photoelectric conversion efficiency, low raw material quality requirements, simple manufacturing process and low energy consumption, the ability to prepare transparent and flexible components, and high weak light efficiency. However, perovskite cells also have the disadvantage of poor stability, which makes them prone to failure. The main reason affecting stability is that perovskite cells are not able to isolate water and oxygen after encapsulation.
[0004] At present, the packaging of perovskite cells mainly uses organic adhesives such as POE / EVA to bond the cover glass and the perovskite conductive glass substrate. However, under the continuous erosion of harsh outdoor weather (ultraviolet rays, high temperature, high humidity, cold and hot cycles), the organic adhesive is prone to yellowing, the viscosity decreases, and the edge of the package is leaking and leaking, which eventually leads to the failure of the perovskite cell. This is also an important reason why the commercialization progress of perovskite cells is currently hindered.
[0005] In order to better solve the problem of perovskite battery packaging, many manufacturers have begun to try glass laser welding solutions. The glass laser welding solution uses ultrafast lasers to directly weld the edges of two pieces of glass to achieve ultra-high water and oxygen barriers. Because no solder is used, it has long-term stability and is an ideal solution for perovskite battery packaging.
[0006] However, laser welding has high requirements for the glass to be welded. When the conductive substrate of the perovskite cell is FTO glass, since FTO glass is a fluorine-doped tin dioxide transparent conductive glass, its surface is coated with a fluorine-doped tin dioxide film layer, which is difficult to remove. As a result, laser welding of FTO glass may cause welding failure. Summary of the invention
[0007] Based on this, the first aspect of the present application provides a method for removing film from FTO glass, and its technical solution is as follows:
[0008] A method for removing film from FTO glass comprises the following steps:
[0009] Prepare a zinc plate according to the shape and size of the film removal area of the FTO glass;
[0010] The FTO glass, zinc plate and hydrochloric acid in the film removal area are brought into contact with each other to react so as to remove the film layer on the surface of the film removal area of the FTO glass.
[0011] The second aspect of the present application provides a method for preparing a perovskite battery, and its technical solution is as follows:
[0012] A method for preparing a perovskite battery comprises the following steps:
[0013] The film removal area of the FTO glass is removed according to the film removal method as described above, and a perovskite cell functional layer is formed on the non-film removal area of the FTO glass;
[0014] The FTO glass after film removal is welded to the cover glass by laser welding to encapsulate the functional layer of the perovskite cell.
[0015] A third aspect of the present application provides a perovskite cell, which is prepared by the preparation method as described above.
[0016] Compared with the traditional solution, this application has the following beneficial effects:
[0017] The present application utilizes zinc plate and hydrochloric acid to remove the film from FTO glass, wherein when the film layer on the surface of the FTO glass, the zinc plate and the hydrochloric acid come into contact with each other, the following reaction occurs: SnO2+Zn+4HCl=SnCl2+ZnCl2+2H2O, the above reaction utilizes the extremely strong reducing property of Zn and the product H2 of Zn and HCl in the reaction process, reducing the +4-valent Sn to +2-valent Sn, and the +2-valent Sn is extremely unstable and cannot bind O atoms, thus being dissolved by hydrochloric acid, achieving the purpose of removing the film from the FTO glass. The above method can be used to remove the fluorine-doped tin dioxide film layer on the FTO glass, and the glass substrate is not damaged after the film layer is removed. The optical transmittance and reflectivity of the glass in the film removal area after the film removal are the same as those of the original glass before the film removal. The above method can realize the mass production removal of the fluorine-doped tin dioxide film layer in FTO glass, which is conducive to the subsequent use of laser welding method to encapsulate the perovskite battery, thereby converting the perovskite battery sealing from organic packaging to inorganic packaging, so that the perovskite battery can almost completely block water vapor (liquid, gas), which will bring the subsequent industrial application of perovskite batteries to a higher level. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0019] Figure 1 A schematic flow chart of a method for removing a film from FTO glass according to an embodiment of the present invention;
[0020] Figure 2Schematic diagram of the structure of FTO glass according to one embodiment;
[0021] Figure 3 It is a schematic structural diagram of a zinc plate according to one embodiment;
[0022] Figure 4 is a schematic diagram of a three-dimensional structure of a fixture according to an embodiment;
[0023] Figure 5 for Figure 4 A schematic diagram of a top view structure of a fixture;
[0024] Figure 6 for Figure 4 A schematic diagram of the front structure of the fixture;
[0025] Figure 7 It is a schematic diagram of a partial structure and a cross-sectional structure after the FTO glass and zinc plate enter the placement space;
[0026] Figure 8 A schematic diagram of immersing the FTO glass and the zinc plate in the film removal area fixedly contacted by the jig into a hydrochloric acid tank;
[0027] Fig. 9 A schematic diagram of a process for preparing a perovskite battery according to an embodiment of the present invention;
[0028] Fig.10 A schematic diagram of the structural transformation of each step of a method for preparing a perovskite battery according to an embodiment;
[0029] Fig.11 A real-life diagram of a perovskite cell according to one embodiment. DETAILED DESCRIPTION
[0030] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0032] the term
[0033] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0034] In the present application, "plurality", "multiple", "multiple times", "plurality", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0035] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0036] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0037] In the present application, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution within the above numerical interval is deemed to be continuous and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), and every numerical value between the two numerical endpoints.
[0038] FTO glass is a fluorine-doped tin dioxide transparent conductive glass with the advantages of high visible light transmittance, low resistivity, and strong acid and alkali resistance. It is used as a conductive substrate for perovskite solar cells. The fluorine-doped tin dioxide film layer in FTO glass is formed by directly coating the fluorine-doped tin dioxide when the glass is formed and not cooled. The presence of this film layer is the main factor leading to the failure of laser welding. The tin dioxide in the fluorine-doped tin dioxide film layer is a relatively stable substance. It is insoluble in acid and alkali at room temperature and pressure, and cannot directly react with reducing substances such as alkali metals and hydrogen at room temperature and pressure. And because the tin dioxide material is also relatively hard, if it is removed by polishing materials, the fallen tin dioxide material will scratch the glass, making the glass unable to be welded using laser. Therefore, how to remove the fluorine-doped tin dioxide film layer on the FTO surface is the key to achieving FTO laser welding.
[0039] The first aspect of the present application provides a method for removing film from FTO glass, see Figure 1 In one embodiment, the method for removing the film of FTO glass comprises the following steps:
[0040] S10. Prepare a zinc plate according to the shape and size of the film removal area of the FTO glass.
[0041] It can be understood that, according to the shape and size of the film removal area of the FTO glass, a zinc plate having the same shape and size as the film removal area can be prepared in a ratio of 1:1. In addition, if the film removal area of the FTO glass includes several sub-areas of the same shape and size, a zinc plate can be prepared in a ratio of 1:1 according to the shape and size of the sub-areas, and the film removal can be completed in each sub-area by reusing the zinc plate. In addition, zinc plates of specific sizes and shapes can be prepared flexibly, such as preparing at least one zinc plate for repeated use or preparing multiple zinc plates to ensure that the zinc plate fully covers the film removal area of the FTO glass. At this time, it is allowed to reuse at least one zinc plate or to use multiple zinc plates to repeatedly remove the film of part of the film removal area.
[0042] In this implementation, see Figure 2 The FTO glass 10 is square, including a film removal area 11 and a non-film removal area 12. The film removal area 11 is located at the edges of the four sides of the FTO glass 10 and surrounds the non-film removal area 12. The width of the film removal area 11 remains unchanged, wherein the width of the film removal area refers to the distance between the non-film removal area 12 and the edge of the FTO glass 10. The structure of the zinc plate in this embodiment is shown in FIG. Figure 3 The length of the zinc plate is consistent with the side length of the FTO glass, and the width of the zinc plate is the same as the width of the film removal area 11. Optionally, the thickness of the zinc plate is 1 mm to 2 mm.
[0043] S20, making the FTO glass, the zinc plate and the hydrochloric acid in the film removal area contact each other and react to remove the film layer on the surface of the film removal area of the FTO glass.
[0044] The above method uses zinc plate and hydrochloric acid to remove the film from FTO glass, wherein when the film layer on the surface of the FTO glass, the zinc plate and the hydrochloric acid come into contact with each other, the following reaction occurs: SnO2+Zn+4HCl=SnCl2+ZnCl2+2H2O, and the above reaction utilizes the extremely strong reducing property of Zn and the product H2 of Zn and HCl in the reaction process to reduce the +4-valent Sn to +2-valent Sn, and the +2-valent Sn is extremely unstable and cannot bind O atoms, so it is dissolved by hydrochloric acid, thereby achieving the purpose of removing the film from the FTO glass. The above method can remove the fluorine-doped tin dioxide film layer on the FTO glass, and the glass substrate is not damaged after the film layer is removed. The optical transmittance and reflectivity of the glass in the film removal area after the film removal are the same as those of the original glass before the film removal. The above method can realize the mass production removal of the fluorine-doped tin dioxide film layer in FTO glass, which is conducive to the subsequent use of laser welding method to encapsulate the perovskite battery, thereby converting the perovskite battery sealing from organic packaging to inorganic packaging, so that the perovskite battery can almost completely block water vapor (liquid, gas), which will bring the subsequent industrial application of perovskite batteries to a higher level.
[0045] Optionally, the FTO glass, the zinc plate and the hydrochloric acid in the film removal area are brought into contact with each other, comprising the following steps:
[0046] S21, preparing a jig, wherein the jig is used to place the FTO glass and the zinc plate so that the FTO glass in the film removal area is in fixed contact with the zinc plate;
[0047] In this implementation, see Figure 4~Figure 6 The fixture 30 includes a frame 31, and the frame 31 includes a first frame 311 and a second frame 312, and a third frame 313 and a fourth frame 314. One end of the third frame 313 is connected to the first frame 313, and the other end is connected to the second frame 312. One end of the fourth frame 314 is connected to the first frame 313, and the other end is connected to the second frame 312. That is, the first frame 311, the second frame 312, the third frame 313 and the fourth frame 314 are connected end to end to enclose a A placement space 32 is formed, a groove 311A is provided on the side wall of the frame 311 near the placement space 32, a groove 312A is provided on the side wall of the frame 312 near the placement space 32, a groove 313A is provided on the side wall of the frame 313 near the placement space 32, and a groove 314A is provided on the side wall of the frame 314 near the placement space 32. The grooves 311A, 312A, 313A and 314A are all through grooves, and the grooves 311A and 312A correspond to each other, and the grooves 313A and 314A correspond to each other. Among them, the grooves 311A and 312A are respectively used to provide an exit and an entrance for the FTO glass to enter and exit the placement space 32. At this time, the FTO glass can enter the placement space 32 by inserting the through groove 311A or 312A, and can leave the placement space 32 by pulling out from the through groove 311A or 312A. The grooves 311A, 312A, 313A and 314A are also used to embed the opposite ends of the FTO glass and the zinc plate, so as to fix the FTO glass and the zinc plate in the placement space and make the film removal area of the FTO glass contact with the zinc plate. Figure 5 , showing that the four edges of the glass 10 are embedded in the grooves 311A, 312A, 313A and 314A to be fixed, and the embedding of the zinc plate is similar, which is not shown in the figure.
[0048] Optionally, along the thickness direction of the frame 31 , the size of the first through groove 311A is not less than the sum of the sizes of the FTO glass and the zinc plate, and the size of the second through groove 312A corresponds to the size of the first through groove 311A, so that the zinc plate and the FTO glass can be placed in the placement space 32 at the same time.
[0049] Optionally, along the thickness direction of the frame 31 , the third through groove 313A is not less than the sum of the sizes of the FTO glass and the zinc plate, and the size of the fourth through groove 314A corresponds to the size of the third through groove 313A, so that the zinc plate and the FTO glass can be placed in the placement space 32 at the same time.
[0050] In other embodiments, the grooves 311A and 312A can also be used alone to embed the opposite ends of the FTO glass and the zinc plate, so as to fix the FTO glass and the zinc plate in the placement space, and make the film removal area of the FTO glass contact the zinc plate. The grooves 313A and 314A can also be used alone to embed the opposite ends of the FTO glass and the zinc plate, so as to fix the FTO glass and the zinc plate in the placement space, and make the film removal area of the FTO glass contact the zinc plate.
[0051] In this embodiment, the groove bodies 311A, 312A, 313A and 314A are all through grooves. In other embodiments, the groove bodies 311A and 312A are through grooves, and the groove bodies 313A and 314A are blind grooves.
[0052] In other embodiments, a plurality of grooves are provided on the side wall of the frame 31 near the placement space 32, at least one of which is a through groove, and the through groove is used to provide an entrance and exit for the FTO glass to enter and exit the placement space, and at least one of the grooves is used to embed the edge of the FTO glass and at least one of the grooves is used to embed the edge of the zinc plate, so as to fix the FTO glass and the zinc plate in the placement space and make the film removal area of the FTO glass contact the zinc plate. For example, the groove 311A is a through groove, which is used to provide an entrance and exit for the FTO glass to enter and exit the placement space, and is also used to embed the edges of the FTO glass and the zinc plate.
[0053] In this embodiment, the fixture 30 is designed according to the shape of the FTO glass 10, and the placement space 32 formed by the frame 31 is square. Figure 7 , which is a partial structure and a cross-sectional structure diagram after the FTO glass 10 and the zinc plate 20 enter the placement space, it can be seen that the FTO glass 10 and the zinc plate 20 are fixedly contacted in the placement space of the fixture 30. It can be understood that the zinc plate 20 can be inserted into the through groove into the placement space 32 first, and then the FTO glass 10 can be inserted into the through groove into the placement space 32, or the FTO glass 10 can be inserted into the through groove 33 into the placement space 32 first, and then the zinc plate 20 can be inserted into the through groove 33 into the placement space.
[0054] It is understandable that the fixture needs to be made of a material that is resistant to acid, alkali and electrochemical corrosion. Optionally, the material of the fixture includes at least one of polytetrafluoroethylene (PTFE), polypropylene (PP) and polyvinyl chloride (PVC). PTFE is preferred.
[0055] Optionally, before the FTO glass, zinc plate and hydrochloric acid in the film removal area are brought into contact with each other, the FTO glass and zinc plate are cleaned. For example, a flat cleaning machine or an ultrasonic tank cleaning machine is used to clean the FTO glass and zinc plate respectively.
[0056] S22. Immerse the FTO glass and zinc plate in the film removal area in fixed contact into hydrochloric acid.
[0057] Optionally, the hydrochloric acid is provided by a hydrochloric acid aqueous solution, and the mass concentration of the hydrochloric acid in the hydrochloric acid aqueous solution is 5% to 20%. For example, the mass concentration of the hydrochloric acid in the hydrochloric acid aqueous solution is 5%, 10%, 15%, or 20%.
[0058] Sn in SnO2 is +4, which is a stable valence state. This oxide is insoluble in water, acid and alkali at room temperature and pressure, and does not react with water, acid and alkali. When the film layer, zinc plate and hydrochloric acid on the surface of FTO glass come into contact with each other, the following reaction will occur: SnO2+Zn+4HCl=SnCl2+ZnCl2+2H2O. The above reaction uses the extremely strong reducing property of Zn and the product H2 of Zn and HCl in the reaction process to reduce +4-valent Sn to +2-valent Sn. +2-valent Sn is extremely unstable and cannot bind O atoms, so it is dissolved by hydrochloric acid, achieving the purpose of FTO glass film removal. In addition, the FTO glass substrate is not damaged after the film layer is removed, and the optical transmittance and reflectivity of the glass in the film removal area after film removal are the same as those of the original glass before film removal.
[0059] Moreover, the reaction between the film layer on the surface of the FTO glass, the zinc plate and the hydrochloric acid can be carried out at room temperature and pressure, without heating at high temperature or in a closed environment, and the reaction conditions are more suitable for industrial large-scale production. If the zinc plate is replaced with an aluminum plate or reducing solid C or reducing gas H2, it is necessary to heat at high temperature or in a closed environment to reduce SnO2 to SnO or Sn soluble in hydrochloric acid, and the reaction conditions are relatively harsh.
[0060] In addition, the reaction products of the film layer on the surface of the FTO glass, the zinc plate and the hydrochloric acid are environmentally friendly and easy to handle. Specifically, the reaction products are mainly SnCl2 and ZnCl2, which can be easily recovered by electrolysis or by using lime to generate precipitated hydroxides, and then high-temperature roasting of the hydroxides to form recyclable oxides.
[0061] The hydrochloric acid can be placed in a hydrochloric acid tank in advance, and the FTO glass and the zinc plate in the film removal area fixedly contacted by the jig are immersed in the hydrochloric acid in the hydrochloric acid tank. Figure 8, is a schematic diagram of immersing the FTO glass and zinc plate in the film removal area that are fixedly contacted by a jig into a hydrochloric acid tank in this embodiment, wherein, as described above, the jig 30 fixes the film removal area of the FTO glass 10 in contact with the zinc plate 20, and the jig 30 together with the FTO glass 10 and the zinc plate 20 in the film removal area at the bottom are immersed in the hydrochloric acid tank 40. At this time, after being immersed in the hydrochloric acid tank 40, the depth of the hydrochloric acid immersion is consistent with the width of the zinc plate 20.
[0062] It can be understood that when the FTO glass in the film removal area is fixedly contacted with the zinc plate, if the shape and size of the zinc plate are exactly the same as those of the film removal area, the zinc plate can completely cover the film removal area, and then the FTO glass in the film removal area and the zinc plate in fixed contact are immersed in hydrochloric acid to complete the removal of the surface film layer in the film removal area of the FTO glass. In addition, if multiple zinc plates are needed or at least one zinc plate needs to be reused to completely cover the film removal area, then each time the zinc plate is used, the zinc plate is fixedly contacted with the FTO glass in the film removal area, and the FTO glass in the film removal area and the zinc plate in fixed contact are immersed in hydrochloric acid, that is, step S21 to step S22 are repeated until the surface film layer in the film removal area of the FTO glass is completely removed. For example, in this embodiment, the same zinc plate 20 is reused, and the zinc plate 20 is fixedly contacted with the film removal area (four edges) of the FTO glass 10 for 4 consecutive times, and the FTO glass in the film removal area and the zinc plate in fixed contact are immersed in hydrochloric acid for 4 consecutive times to remove the film so that the surface film layer in the film removal area of the FTO glass is completely removed.
[0063] Considering that the reaction process of the FTO glass film layer, the zinc plate and the hydrochloric acid, especially the reaction end point, is not easy to monitor. Optionally, after preparing the zinc plate, the following steps are also included:
[0064] Prepare a power supply, connect the zinc plate to the positive electrode of the power supply, and connect the FTO glass to the negative electrode of the power supply;
[0065] When the FTO glass, the zinc plate and the hydrochloric acid in the film removal area are in contact with each other, the power supply is kept in an energized state.
[0066] After the FTO glass is connected to the negative electrode of the power supply, since the FTO glass itself is a conductive glass, it is equivalent to the SnO2 film layer on the surface of the FTO glass being connected to the negative electrode. During the power-on process, Zn 2+ , H + Move to SnO2, Zn 2+ It is reduced to Zn in the negative electrode electrolysis. Zn can undergo reduction reaction with SnO2 in the presence of hydrochloric acid and electricity. In this process, the following reactions occur: Zn+SnO2=ZnO+SnO, ZnO+2HCl=ZnCl+H2O, SnO+2HCl=SnCl2+H2O.
[0067] By connecting to the power supply, not only can the reaction progress of the FTO glass film layer, zinc plate and hydrochloric acid be monitored by monitoring the current, but the reaction time can also be shortened and the film removal efficiency can be improved through potential induction.
[0068] After the reaction is completed, the jig is lifted out of the hydrochloric acid tank to remove the FTO glass and zinc plate in the fixed contact film removal area from the hydrochloric acid. It can be understood that before taking the FTO glass and zinc plate out of the jig, the whole can be immersed in a clean water tank for cleaning to remove the reaction residues. After cleaning, the FTO glass and zinc plate are taken out of the jig.
[0069] The above method removes the fluorine-doped tin dioxide film layer in the FTO glass without damaging the glass substrate, and the optical transmittance and reflectivity of the glass in the removed area after the film removal are the same as those of the original glass before the film removal. The above method can achieve mass production removal of the fluorine-doped tin dioxide film layer in the FTO glass, which is conducive to the subsequent use of laser welding methods to encapsulate the perovskite battery, thereby converting the perovskite battery sealing from organic packaging to inorganic packaging, and making the perovskite battery almost completely blocked from water vapor (liquid, gas), which is a step up for the subsequent industrial application of perovskite batteries.
[0070] The second aspect of the present application provides a method for preparing a perovskite battery. Fig. 9 In one embodiment, the method for preparing a perovskite cell comprises the following steps:
[0071] S30, removing the film from the film removal area of the FTO glass according to the film removal method as described above, and forming a perovskite cell functional layer on the non-film removal area of the FTO glass.
[0072] In this implementation, see Fig.10 After the film removal area of the FTO glass 10 is removed, the perovskite cell functional layer 50 is formed on the non-film removal area of the FTO glass 10.
[0073] S40, welding the FTO glass after film removal to the cover glass by laser welding to encapsulate the functional layer of the perovskite battery.
[0074] In this implementation, see Fig.10 The FTO glass 10 in the film removal area is welded to the cover glass 60 by laser welding to encapsulate the perovskite cell functional layer 50. The actual picture of the perovskite cell prepared in this embodiment is as follows: Fig.11 shown.
[0075] Optionally, after film removal and before laser welding, the following step is further included: polishing the film removal area of the FTO glass after film removal. Since the film layer on the surface of the FTO glass is a fluorine-doped tin dioxide film layer, after the film removal and tin dioxide removal, in order to achieve the conditions for laser welding, the film removal area of the FTO glass after film removal is subjected to optical-grade polishing, and foreign matter and bumps in the film removal area are polished clean to prevent impurities from causing welding failure.
[0076] It is understandable that the polishing process can be done manually or mechanically. For example, a brush is installed on a fine engraving machine for mechanical polishing. After polishing, the polishing area is cleaned.
[0077] Optionally, the polishing process is completed by using a polishing liquid. Optionally, the polishing liquid includes polishing powder and a solvent. Optionally, the particle size of the polishing powder is 0.5 μm to 2 μm. Optionally, the solvent is water. Optionally, the specific gravity of the polishing powder in the polishing liquid is 0.8 to 1.5.
[0078] It can be understood that the laser welding instrument is a femtosecond infrared laser. Before laser welding, the glass is clamped by a clamping device, such as a clamp, a cylinder pressing fixture, etc. Optionally, the frequency of the laser welding is 50KHz~2MHz. Optionally, the power range of the laser welding is 0.5W~6W or the energy percentage is 5%~100%.
[0079] A third aspect of the present application provides a perovskite cell, which is prepared by the preparation method as described above.
[0080] The following is further described in conjunction with specific embodiments. The raw materials involved in the following specific embodiments, unless otherwise specified, can all be commercially available. The instruments used, unless otherwise specified, can all be commercially available. The processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0081] Example 1
[0082] This embodiment provides a method for preparing a perovskite battery, the steps are as follows:
[0083] S10. Prepare Figure 2 FTO glass of the structure shown, Figure 3 The zinc plate of the structure shown, Figure 4~Figure 6 A fixture of the structure shown.
[0084] S20, inserting the FTO glass and the zinc plate into a jig, and inserting the jig into a hydrochloric acid tank, so that the FTO glass, the zinc plate and the hydrochloric acid in the film removal area are in contact with each other and react, until the film layer in the film removal area of the FTO glass is completely removed, thereby obtaining the FTO glass after film removal.
[0085] S30, forming a perovskite cell functional layer in the non-film removal area of the FTO glass.
[0086] S40, using laser welding to weld the FTO glass in the film removal area to the cover glass to encapsulate the functional layer of the perovskite battery to obtain a perovskite battery.
[0087] After laser welding, it was observed that there were no rainbow patterns or cracks on the four sides of the perovskite battery except for the film area (welding area), indicating complete welding. Two perovskite battery samples were taken and subjected to high temperature and high humidity and water boiling for 720 hours (30 days) respectively. It was found that no water vapor entered the internal perovskite battery area, indicating that it was completely sealed.
[0088] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0089] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for removing film from FTO glass, characterized in that: The following steps are involved: Prepare a zinc plate according to the shape and size of the film removal area of the FTO glass; The FTO glass, the zinc plate and the hydrochloric acid in the film removal area are brought into contact with each other to react with each other, so as to remove the film layer on the surface of the film removal area of the FTO glass.
2. The method for removing film from FTO glass according to claim 1, wherein: The FTO glass, the zinc plate and the hydrochloric acid in the film removal area are brought into contact with each other, comprising the following steps: Preparing a jig for placing the FTO glass and the zinc plate so that the FTO glass in the film removal area is in fixed contact with the zinc plate; Immerse the FTO glass and zinc plate in the film removal area in fixed contact in hydrochloric acid.
3. The method for removing film from FTO glass according to claim 2, wherein: The jig includes a frame, which is configured to enclose a placement space. A plurality of grooves are provided on the side wall of the frame close to the placement space, at least one of which is a through groove, which is used to provide an entrance and exit for the FTO glass to enter and exit the placement space. At least one of the grooves is used to embed the edge of the FTO glass and at least one of the grooves is used to embed the edge of the zinc plate, so as to fix the FTO glass and the zinc plate in the placement space and make the film removal area of the FTO glass contact the zinc plate.
4. The method for removing film from FTO glass according to claim 2, wherein: The material of the fixture includes at least one of PTFE, PP and PVC.
5. The method for removing film from FTO glass according to claim 1, wherein: After the zinc plate is prepared, the following steps are also included: Prepare a power supply, connect the zinc plate to the positive electrode of the power supply, and connect the FTO glass to the negative electrode of the power supply; When the FTO glass, the zinc plate and the hydrochloric acid in the film removal area are in contact with each other, the power supply is kept in an energized state. 6 . The method for removing film from FTO glass according to claim 1 , wherein the thickness of the zinc plate is 1 mm to 2 mm.
7. The method for removing film from FTO glass according to any one of claims 1 to 5, wherein the hydrochloric acid is provided by a hydrochloric acid aqueous solution, and the mass concentration of hydrochloric acid in the hydrochloric acid aqueous solution is 5% to 20%.
8. A method for preparing a perovskite battery, characterized in that: The following steps are involved: De-filming the FTO glass in the de-filming area according to any one of claims 1 to 7, and forming a perovskite cell functional layer on the non-de-filming area of the FTO glass; The FTO glass after film removal is welded to the cover glass by laser welding to encapsulate the functional layer of the perovskite cell.
9. The method for preparing a perovskite battery according to claim 8, further comprising the following steps after film removal and before laser welding: The film-removed area of the FTO glass after film removal is polished.
10. A perovskite battery, characterized in that: It is prepared by the preparation method according to any one of claims 8 to 9.
Citation Information
Patent Citations
Method for etching FTO (fluorine-doped tin oxide) conductive thin film
CN103422153A
Method for etching FTO conductive thin film
CN103435266A
Perovskite solar cell packaging method and perovskite solar cell
CN115581106A
Process and device for etching a thin conducting layer deposited on an insulating plate, so as to form an array of electrodes thereon
CN1572009A
Treatment of electroconductive films
GB724088A