Preparation method of cement clinker and cement material

By using a mixed atmosphere of oxygen and carbon dioxide under oxygen-rich combustion conditions during cement clinker calcining, the problem of high NOx generation and low C3S content in traditional cement clinker is solved, and the performance and carbon capture efficiency of cement clinker are improved. , realizes a low-carbon and environmentally friendly production process.

CN118954985APending Publication Date: 2024-11-15CHINA BUILDING MATERIALS ACADEMY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411288047.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the traditional cement clinker calcining process, the NOx generation amount is high, the carbon capture and storage is difficult, and the C3S content in clinker is low, resulting in poor clinker performance.

Method used

Use cement clinker under oxygen-rich combustion conditions, and use a specific proportional mixture atmosphere of oxygen and carbon dioxide (volume ratio 0.21-0.61: 0.39-0.79), to change the fuel combustion mechanism, improve the carbonate decomposition rate, and promote the C2S to C3S. Transform, reduce NOx generation, and improve the C3S content and performance of clinker.

Benefits of technology

It significantly improves the content and performance of C3S in cement clinker, reduces the generation of pollutant NOx, simplifies the carbon capture and storage process, improves the compressive strength and hydration effect of clinker, and reduces carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954985A_ABST
    Figure CN118954985A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of cement materials, and particularly relates to a preparation method of cement clinker and a cement material. The preparation method of the cement clinker provided by the invention comprises the following steps: 1) preparing a cement raw material; and 2) calcining the cement raw material in an oxygen-enriched atmosphere, wherein the oxygen-enriched atmosphere is a mixed gas of oxygen and carbon dioxide in a volume ratio of (0.21-0.61): (0.39-0.79). According to the preparation method of the cement clinker disclosed by the invention, a pollutant NOx is not easy to generate, CO2 is mainly contained in flue gas, so that carbon capture and storage are facilitated, and the prepared cement clinker is high in C3S content and good in performance (hydration effect and stability).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cement materials, and in particular relates to a method for preparing cement clinker and a cement material. Background Art

[0002] Cement clinker, as a semi-finished product of cement, is a key step in cement production. Cement clinker is made of limestone, clay and iron raw materials as the main raw materials, which are prepared into raw materials in appropriate proportions and formed into cement clinker through calcination.

[0003] The traditional cement clinker calcining process uses air as the calcining atmosphere. The temperature in the kiln is relatively low, and the carbonate decomposition rate in the raw materials is low, resulting in a low conversion rate of 2CaO·SiO2 (C2S) to 3CaO·SiO2 (C3S) during the clinker calcining process. The C3S content in the formed clinker is low, which is not conducive to improving the quality of the clinker. In addition, air is not conducive to the complete combustion of the fuel. N2 and inert gases, which account for about 79% of the air, not only cannot play a role in supporting combustion, but also lead to the formation of pollutants such as NO. x The amount of CO2 generated increases, and the volume fraction of CO2 in the calciner is low, which makes carbon capture and storage difficult. Summary of the invention

[0004] Therefore, the present invention provides a method for preparing cement clinker under oxygen-enriched combustion conditions, which aims to solve the problem of NO pollutants in the existing cement clinker production process to a certain extent. x Problems include high generation volume, difficulty in carbon capture and storage, low C3S content in cement clinker, and poor clinker performance.

[0005] The present invention also provides cement clinker prepared by the method and cement material containing the same.

[0006] The present invention provides a method for preparing cement clinker, comprising the following steps:

[0007] 1) Prepare cement raw material;

[0008] 2) calcining the cement raw material in an oxygen-rich atmosphere, wherein the oxygen-rich atmosphere is a mixed gas of oxygen and carbon dioxide in a volume ratio of (0.21-0.61):(0.39-0.79).

[0009] Preferably, the volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 21%-50%.

[0010] Preferably, the volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 31% or 41%.

[0011] Preferably, in step 2), the calcination temperature is 1430° C.-1470° C., and the calcination time is 45 min-75 min.

[0012] Preferably, the raw material composition of the cement raw material in step 1) includes, by weight, 75-85 parts of limestone, 5-15 parts of coal-fired slag, 1-5 parts of iron ore tailings powder and 5-10 parts of gas ash.

[0013] Preferably, the raw material composition of the cement raw material in step 1) also includes fly ash;

[0014] The added amount of the fly ash accounts for 0.8%-4% of the total mass of the cement raw material.

[0015] Optionally, the coal ash of the present invention is obtained by burning coal powder to 815°C;

[0016] Optionally, the cement raw material powder used to prepare the cement raw meal in step 1) has a particle size of 80 μm and a sieve residue of 4%-6%.

[0017] The present invention provides a cement clinker which is prepared by adopting the above-mentioned method for preparing the cement clinker.

[0018] Preferably, the cement clinker comprises the following mineral phases, measured in percentage by mass: C3S 58%-70%, C2S 10%-17%, C3A 2.0%-2.7%, C4AF 17%-23% and the remainder of miscellaneous mineral phases.

[0019] Preferably, the cement clinker comprises the following mineral phases in terms of mass percentage: C3S 69.1%, C2S 11.4%, C3A 2.0%, C4AF 17.4% and the remainder of miscellaneous mineral phases;

[0020] Alternatively, C3S 63.3%, C2S 14.2%, C3A 2.0%, C4AF 20.4% and the remainder of miscellaneous mineral phases.

[0021] The present invention also provides a cement material, comprising the above-mentioned cement clinker.

[0022] The technical solution of the present invention has the following advantages:

[0023] 1. The method for preparing cement clinker provided by the present invention comprises the following steps: 1) preparing cement raw material; 2) calcining the cement raw material in an oxygen-rich atmosphere, wherein the oxygen-rich atmosphere is a mixture of oxygen and carbon dioxide in a volume ratio of (0.21-0.61): (0.39-0.79). The preparation method of the present invention changes the equilibrium partial pressure of CO2 in the system and the fuel combustion mechanism by calcining in an oxygen-rich atmosphere with a specific ratio of oxygen and carbon dioxide without changing the composition and ratio of the cement raw material. With the addition of CO2, the activation energy and pre-exponential factor of the fuel combustion reaction are reduced, the reaction rate constant is reduced, thereby increasing the combustion peak span time, effectively reducing the coal consumption in the clinker calcination, increasing the cement clinker output, and at the same time increasing the carbonate decomposition rate in the raw material, promoting the conversion of C2S to C3S, which is conducive to the generation of more C3S in the cement clinker, and the prepared clinker has a better submicroscopic morphology, wherein the Alite (main component of which is C3S) crystal size becomes larger, the boundary is clearer, the crystal morphology is excellent, and more CSH gels and needle-shaped crystals appear on the surface of the hydration product; using an oxygen-rich atmosphere with a specific ratio of oxygen and carbon dioxide for calcination can significantly reduce the pollutant NO x The flue gas after calcination is mainly CO2, which reduces the difficulty of separation and makes carbon capture and storage easier. The preparation method of cement clinker of the present invention is not easy to generate pollutants NO x The flue gas is mainly CO2, which is more conducive to carbon capture and storage. The prepared cement clinker has a high C3S content and good cement clinker performance (hydration effect, stability).

[0024] 2. In the method for preparing cement clinker provided by the present invention, preferably, the volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 21%-50%. By controlling the volume percentage of oxygen in the oxygen-enriched atmosphere to 21%-50%, the compressive strength of the obtained cement clinker is significantly improved. Further preferably, the volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 31% or 41%. An oxygen-enriched atmosphere with a specific ratio of oxygen and carbon dioxide is selected for calcination, and the obtained cement clinker has good performance (hydration effect, stability), and at the same time, the compressive strength of the cement clinker is higher and the quality of the cement clinker is better.

[0025] 3. The method for preparing cement clinker provided by the present invention can reduce the clinker coefficient when producing cement of the same strength grade using the prepared cement clinker, thereby reducing carbon emissions in the cement production process, which is beneficial to the low-carbon transformation of the cement industry.

[0026] 4. The preparation method of cement clinker provided by the present invention is efficient, low-carbon, environmentally friendly, and the process is simple and easy to implement, with high environmental and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 XRD comparison diagram of cement clinker of Examples 1-5 of the present invention and Comparative Example 1;

[0029] Figure 2 Comparison of the mass content of free calcium oxide (f-CaO) in cement clinker of Examples 1-5 of the present invention and Comparative Example 1;

[0030] Figure 3 Comparison of 3-day and 28-day compressive strength of cement containing cement clinker of Examples 1-5 and Comparative Example 1 of the present invention;

[0031] Figure 4 Polarized light microscope comparison of cement clinker of Example 1 (A1), Example 2 (A2) and Comparative Example 1 (A0) of the present invention (wherein Alite is Alite crystal and Belite is Belite crystal);

[0032] Figure 5 Polarized light microscope comparison of cement clinker of Example 3 (A3), Example 4 (A4) and Example 5 (A5) of the present invention (wherein Alite is Alite crystal and Belite is Belite crystal);

[0033] Figure 6 Scanning electron microscope comparison of cement clinker after hydration of Example 1 (A1), Example 2 (A2) and Comparative Example 1 (A0) of the present invention;

[0034] Figure 7 Scanning electron microscope comparison of cement clinker after hydration of Example 3 (A3), Example 4 (A4) and Example 5 (A5) of the present invention. DETAILED DESCRIPTION

[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0037] The components of the limestone used in the embodiments of the present invention and the comparative examples include: CaO 48.24%, SiO2 5.76%, Al2O3 1.46%, Fe2O3 0.70%, MgO 1.78%, SO3 0.30%, K2O 0.43%, Na2O 0.08%, and loss on ignition 41.25%;

[0038] The composition of coal-fired slag includes: CaO 5.17%, SiO2 62.01%, Al2O3 21.87%, Fe2O34.13%, MgO 0.26%, SO3 0.03%, K2O 2.56%, Na2O 1.07%, loss on ignition 2.90%;

[0039] The composition of iron tailings powder includes: CaO 2.02%, SiO2 79.41%, Al2O3 3.20%, Fe2O39.77%, MgO2.04%, SO3 0.28%, K2O 0.59%, Na2O 0.23%, loss on ignition 2.46%; Source: Anshan Jinhe Mining Co., Ltd.;

[0040] The components of gas ash include: CaO 5.43%, SiO2 10.37%, Al2O3 5.75%, Fe2O334.96%, MgO1.59%, SO3 0.13%, K2O 0.91%, Na2O 0.39%, and loss on ignition 40.48%.

[0041] Example 1

[0042] This embodiment provides a method for preparing cement clinker, comprising the following steps:

[0043] 1) According to the raw material composition of cement raw material, 81.34% limestone, 7.94% coal-fired slag, 1.98% iron tailing powder, 7.93% gas ash and 0.81% coal ash are mixed to prepare cement raw material, wherein the coal ash is obtained by burning bituminous coal powder to 815° C., and the powder particle size of limestone, coal-fired slag, iron tailing powder, gas ash and coal ash is 80 μm and the sieve residue is 5%;

[0044] 2) calcining the cement raw material in an oxygen-rich atmosphere, wherein the oxygen-rich atmosphere is a mixed gas of oxygen and carbon dioxide in a volume ratio of 0.61:0.39, the calcination temperature is 1450° C., and the calcination time is 75 min, to obtain the cement clinker.

[0045] Example 2

[0046] This embodiment provides a method for preparing cement clinker, which is different from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.51:0.49.

[0047] Example 3

[0048] This embodiment provides a method for preparing cement clinker, which is different from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.41:0.59.

[0049] Example 4

[0050] This embodiment provides a method for preparing cement clinker, which is different from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.31:0.69.

[0051] Example 5

[0052] This embodiment provides a cement clinker method, which is different from the embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.21:0.79.

[0053] Example 6

[0054] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.41:0.59, the calcination temperature is 1430° C., and the calcination time is 75 min.

[0055] Example 7

[0056] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.31:0.69, the calcination temperature is 1430° C., and the calcination time is 60 min.

[0057] Example 8

[0058] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.21:0.79, the calcination temperature is 1430° C., and the calcination time is 75 min.

[0059] Example 9

[0060] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.41:0.59, the calcination temperature is 1450° C., and the calcination time is 45 min.

[0061] Example 10

[0062] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.21:0.79, the calcination temperature is 1450° C., and the calcination time is 45 min.

[0063] Embodiment 11

[0064] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.61:0.39, the calcination temperature is 1450° C., and the calcination time is 60 min.

[0065] Example 12

[0066] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.51:0.49, the calcination temperature is 1450° C., and the calcination time is 60 min.

[0067] Embodiment 13

[0068] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.31:0.69, the calcination temperature is 1470°C, and the calcination time is 45 minutes.

[0069] Embodiment 14

[0070] This embodiment provides a method for preparing cement clinker, which differs from the method of embodiment 1 only in that the oxygen-enriched atmosphere in step 2) is a mixture of oxygen and carbon dioxide in a volume ratio of 0.41:0.59, the calcination temperature is 1470°C, and the calcination time is 60 min.

[0071] Comparative Example 1

[0072] This comparative example provides a method for preparing cement clinker, which differs from Example 1 only in that in step 2), the cement clinker is placed in a silicon-molybdenum furnace with an adjustable atmosphere and calcined in an air atmosphere at a calcination temperature of 1450° C. for 75 minutes to obtain the cement clinker.

[0073] Test Example 1

[0074] The cement clinker of Examples 1-5 and Comparative Example 1 was scanned using a D8 Advance X-ray diffractometer from Brucker, Germany, under the following test conditions: accelerating voltage 40 kV, accelerating current 40 mA, step length 0.02°, scanning time per step 1 s, scanning angle 10-70°. After scanning, the clinker sample was refined using the Rietveld full spectrum fitting analysis method using the software MAUD. The obtained XRD patterns and refinement results were used to determine the mineral phase content. The analysis results of the mineral phase content of different samples are shown in Table 1. The XRD patterns are shown in Table 1. Figure 1 shown.

[0075] 3CaO·SiO2(C3S), 2CaO·SiO2(C2S), 3CaO·Al2O3(C3A), 4CaO·Al2O3·Fe2O3(C4AF) are the four main mineral phases of cement clinker, and the rest are small amounts of miscellaneous mineral phases. Under different calcination systems, the crystal structure and mineral composition of cement clinker will change significantly. The sample numbers corresponding to Examples 1-5 and Comparative Example 1 are shown in Table 1, which are consistent with the sample numbers in the subsequent test examples.

[0076] Table 1

[0077]

[0078] As can be seen from Table 1, compared with the A0 sample fired in air atmosphere in Comparative Example 1, the C3S content in the sample calcined in the CO2 / O2 mixed oxygen-enriched atmosphere has a significant increase, while C2S, C3A, and C4AF have a significant decrease. With the change of CO2 concentration, the content of C3S and C4AF has changed significantly. It can be seen that the present invention can significantly increase the C3S content in cement clinker by calcining in the CO2 / O2 mixed oxygen-enriched atmosphere.

[0079] In addition, when the CO2 content is low, with the increase of the CO2 / O2 ratio, the C3S content in the calcined sample gradually increases. In Example 3, the C3S content in the A3 sample calcined under the atmosphere of CO2 / O2 ratio reaching 0.59 / 0.41 reaches the highest (69.1%), and then with the increase of CO2 / O2 ratio, the C3S content begins to decline. When the CO2 / O2 ratio reaches 0.79 / 0.21, the C3S content rises again. Obviously, the influence of CO2 / O2 atmosphere on the mineral phase composition in the calcined sample is relatively complex. The most likely reason is the change of the mineral phase and liquid phase formation temperature brought by the CO2 / O2 atmosphere during the combustion process, especially the liquid phase content and properties are crucial to the generation of C3S. The optimal calcination atmosphere is more conducive to the conversion of C2S to C3S, so that the C3S content in the clinker is the highest. From the above results, it can be seen that the C3S content in the A3 sample of Example 3 is the highest (69.1%), which indicates that when the CO2 / O2 ratio is 0.59 / 0.41, it is the most favorable calcination atmosphere for the growth of C3S in the clinker.

[0080] Test Example 2

[0081] The free calcium oxide mass content of the cement clinker of Examples 1-5 and Comparative Example 1 was measured using an FC-6 cement free calcium oxide rapid tester. The results are as follows: Figure 2 shown.

[0082] The cement clinkers of Examples 1-5 and Comparative Example 1 were crushed until all of them passed through a 5 mm square hole sieve, and then ground with natural dihydrate gypsum that complies with GB / T5483 in a standard test small mill to prepare P·I type silicate cement, wherein the mass content of natural dihydrate gypsum is 5%. The 3-day and 28-day compressive strengths of P·I type silicate cement were measured in accordance with GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", and the results are as follows: Figure 3 shown.

[0083] Depend on Figure 2It can be seen that the free calcium oxide (f-CaO) content of the sample calcined in air atmosphere is 0.88wt%, and the f-CaO content of all samples calcined in CO2 / O2 atmosphere has decreased. This is because after adding a certain concentration of CO2 to the atmosphere, the equilibrium partial pressure of CO2 in the system is changed, slowing down the decomposition process of carbonates. On the other hand, as the ratio of CO2 / O2 increases from 0.39 / 0.61 to 0.79 / 0.21, the f-CaO content in the clinker shows a significant upward trend. In addition, the f-CaO content of all experimental samples is always lower than 1.0wt%, and all meet the f-CaO control requirements of the clinker. The increase in the free calcium oxide (f-CaO) content in cement clinker will directly affect the stability of cement. It can be seen that the embodiments of the present invention can ensure the stability of cement and improve the quality of cement when calcined in CO2 / O2 atmosphere.

[0084] Depend on Figure 3 It can be seen that the compressive strength of samples A1 to A3 in the embodiment increases, and then the compressive strength of samples A4 and A5 decreases, indicating that a moderate increase in the CO2 / O2 concentration ratio is conducive to improving the compressive strength of cement, that is, it can be reflected that the compressive strength of cement clinker is improved. When the CO2 / O2 ratio reaches 0.59 / 0.41 (sample A3), the strength of cement clinker is the highest; when the CO2 / O2 ratio is further increased, the compressive strength begins to decrease again, but even when the CO2 / O2 ratio is 0.79 / 0.21, the compressive strength of cement clinker is still equivalent to that of sample A0 calcined in a traditional air atmosphere. That is, in Examples 3-5, the cement clinker calcined when the CO2 / O2 concentration ratio is 0.59 / 0.41, 0.69 / 0.31, and 0.79 / 0.21 has high compressive strength and the quality of cement clinker is further improved.

[0085] In addition, it can be observed that sample A4 showed the highest strength growth (79.10%) during the 3-28 days of age, and sample A3 also showed a high strength growth rate (77.32%). The strength growth rates of samples A0, A1, and A2 were similar, all 75.10%, while the strength growth rate of sample A5 was relatively low. These results show that the CO2 calcination atmosphere has an effect on the strength growth of clinker, and the strength growth of cement clinker is the highest when the CO2 / O2 ratio is 0.59 / 0.41 and 0.69 / 0.31.

[0086] In summary, it can be seen that the CO2 calcination atmosphere has an impact on the strength of clinker. When the CO2 / O2 concentration ratio is in the range of 0.39 / 0.61 to 0.79 / 0.21, a moderate increase in the CO2 / O2 concentration is beneficial to improving the compressive strength of cement clinker. When the CO2 / O2 ratio is 0.59 / 0.41 and 0.69 / 0.31, the strength of cement clinker is optimal, and the strength growth within the age of 3-28 days is also the largest.

[0087] Test Example 3

[0088] The cement clinkers of Examples 1-5 and Comparative Example 1 were fixed with phenolic resin and then ground and polished. The sample plane was etched with ammonium chloride solution (wt%=1%), and then the microstructure of the cement clinkers of Examples 1-5 and Comparative Example 1 was observed and analyzed using an Olympus BX-51 polarizing microscope. The polarizing microscope images obtained are as follows: Figure 4 and Figure 5 As shown, two polarizing microscope images at different positions of each sample were selected. Observe under a polarizing microscope. At this time, free calcium oxide will appear colorful. Alite (mainly composed of C3S) crystals are mainly blue or dark brown, with hexagonal or square shapes, and Belite (mainly composed of C2S) crystals are light brown and round in shape.

[0089] Depend on Figure 4 and Figure 5 The submicrostructure of clinker minerals obtained in different calcination atmospheres can be seen. Comparison of the mineral morphology of the six groups of samples under a reflected light microscope shows that when the calcination atmosphere changes from air to CO2 / O2, the number of Alite crystals in the clinker increases, the size becomes larger, and the boundaries become clearer. And with the change of the CO2 / O2 ratio of the calcination atmosphere, the Alite crystals in the clinker become larger in size, with clearer and more complete outlines, while the size of the Belite crystals becomes smaller and the outlines become more blurred. Among all the samples, the crystal morphology of sample A3 is the best. Most of the Alite crystals in the A3 sample are regular and complete in shape, mostly hexagonal plates and short columns, with uniform size and a large number, accounting for about 60%-70%, and with more inclusions; the number of Belite crystals is small, the size is moderate, most of the shapes are oval and egg-shaped, with smooth edges, and a few have crystal lines and cross stripes. In contrast, sample A0 of comparative example has fewer Alite crystals with irregular shapes, uneven sizes, fuzzy edges, and minerals that are mostly stuck together. In the field of vision, it can be seen that the content of Belite crystals is relatively high, with a basic round shape and smooth edges, and C3S scattered in the middle.

[0090] Test Example 4

[0091] The cement clinkers of Examples 1-5 and Comparative Example 1 were hydrated for 3 days respectively. The specific hydration treatment steps included: according to a water-cement ratio of 0.4:1, the cement clinker samples were made into 20mm×20mm×20mm pure slurry test blocks, and after being cured for 1 day at a standard constant temperature and humidity (temperature 20±1°C, humidity 95±1%), the test blocks were demoulded, and further immersed in deionized water at 20±1°C for 2 days. The test blocks were taken out and broken, and anhydrous ethanol was used to terminate the hydration for subsequent testing and analysis; the cement clinker hydrated samples of Examples 1-5 and Comparative Example 1 were characterized by using a field emission scanning electron microscope (UltraPlus, Zeiss), and the crystal size and crystal morphology formed after the cement clinker was hydrated were observed. The obtained scanning electron microscope images are shown in FIG. Figure 6 and Figure 7 As shown, scanning electron micrographs of two different locations were selected for each sample.

[0092] Figure 6 and Figure 7 The figure shows the surface microscopic morphology of the clinker obtained in different calcination atmospheres after hydration (3 days). It can be seen from the image that the surface hydration products of the samples in different calcination atmospheres are basically the same, that is, the early hydration product type I calcium silicate hydrate (CSH), which is a slender substance that grows radially outward from the cement particles. However, the surface hydration products of A0 and A1 are more dispersed, and the mineral sizes are quite different; the A2 sample has lath-shaped and tubular CSH; the mineral distribution of A3 and A4 is uniform and relatively dense, and the gear-shaped and fibrous CSH gels are staggered and stacked, presenting an interlocking mesh structure, indicating that the cement clinker of A3 and A4 samples has a high degree of hydration and a fast hydration rate, which also indirectly indicates that under the CO2 / O2 atmosphere ratio in Examples 3 and 4, the cement compressive strength of A3 and A4 is excellent; the surface hydrated minerals of A5 are dispersed, and it is obvious that there are more gullies and cracks between the minerals. The mineral size is small and the hydration is basically completed. The long strip particles overlap the hydrated spherical particle minerals and are interlaced. However, the A0 sample corresponding to comparative example 1 has a low degree of hydration, and the hexagonal plate and short columnar morphologies are still more numerous.

[0093] Test Example 5

[0094] The free calcium oxide content in the cement clinker of Examples 6-14 was determined using an FC-6 cement free calcium oxide rapid determination instrument; the test results are shown in Table 4.

[0095] The cement clinker of Examples 6-14 was scanned using a D8 Advance X-ray diffractometer from Brucker, Germany, under the following test conditions: accelerating voltage 40 kV, accelerating current 40 mA, step length 0.02°, scanning time per step 1 s, and scanning angle 10-70°. After scanning, the clinker sample was refined using the Rietveld full spectrum fitting analysis method using the software MAUD to determine the mineral phase content; the test results are shown in Table 4.

[0096] The cement clinker of Examples 6-14 was crushed until it all passed through a 5 mm square hole sieve, and then ground with natural dihydrate gypsum that meets the requirements of GB / T5483 in a standard test small mill to prepare P·I type silicate cement, wherein the mass content of natural dihydrate gypsum is 5%. The 3-day and 28-day compressive strengths of P·I type silicate cement were measured in accordance with GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)"; the test results are shown in Table 4.

[0097] The cement clinkers obtained in Example 4 and Examples 6-14 were subjected to petrographic scoring. The petrographic scoring was performed by using an Olympus BX-51 polarizing microscope to observe the microstructure of the clinker. The score was determined based on the porosity, pore size and dimension; mineral content, degree of erosion and uniformity of distribution; crystal shape, dimension and size. The petrographic scoring standards are shown in Table 3, and the test results are shown in Table 4.

[0098] Table 3

[0099]

[0100]

[0101] Table 4

[0102]

[0103] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing cement clinker, characterized in that: The following steps are involved: 1) Prepare cement raw material; 2) calcining the cement raw material in an oxygen-rich atmosphere, wherein the oxygen-rich atmosphere is a mixed gas of oxygen and carbon dioxide in a volume ratio of (0.21-0.61):(0.39-0.79).

2. The method for preparing cement clinker according to claim 1, characterized in that: The volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 21%-50%.

3. The method for preparing cement clinker according to claim 2, characterized in that: The volume percentage of oxygen in the oxygen-enriched atmosphere in step 2) is 31% or 41%.

4. The method for preparing cement clinker according to claim 1, characterized in that: In step 2), the calcination temperature is 1430° C.-1470° C., and the calcination time is 45 min-75 min.

5. The method for preparing cement clinker according to claim 1, characterized in that: The raw material composition of the cement raw material in step 1) includes, by weight, 75-85 parts of limestone, 5-15 parts of coal-fired slag, 1-5 parts of iron ore tailings powder and 5-10 parts of gas ash.

6. The method for preparing cement clinker according to claim 5, characterized in that: The raw material composition of the cement raw material in step 1) also includes fly ash; The added amount of the fly ash accounts for 0.8%-4% of the total mass of the cement raw material.

7. A cement clinker prepared by the method for preparing cement clinker according to any one of claims 1 to 6.

8. The cement clinker according to claim 7, characterized in that: Calculated by mass percentage, the cement clinker comprises the following mineral phases: C3S 58%-70%, C2S 10%-17%, C3A 2.0%-2.7%, C4AF 17%-23% and the remainder of miscellaneous mineral phases.

9. The cement clinker according to claim 8, characterized in that: The cement clinker comprises the following mineral phases in terms of mass percentage: C3S 69.1%, C2S 11.4%, C3A 2.0%, C4AF 17.4% and the remainder of miscellaneous mineral phases; Alternatively, the cement clinker comprises the following mineral phases in terms of mass percentage: C3S 63.3%, C2S 14.2%, C3A 2.0%, C4AF 20.4% and the remainder of miscellaneous mineral phases.