High-strength shrinkage-free lining wall post-grouting material for seabed mining method tunnel

By using high-strength non-shrinkage grouting material in the construction of subsea mine tunnels, using slag powder and alkali excitation materials, combined with permeable crystalline waterproofing materials and plastic expansion agents, the strength, stability and waterproofing performance of the grouting material are solved. It has achieved efficient gap filling and improved sulfate corrosion resistance.

CN118955061APending Publication Date: 2024-11-15CHINA RAILWAY TUNNEL BUREAU TESTING & INSPECTION CO LTD

Patent Information

Application Number
CN202411024343.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the construction of submarine mine tunnels, the existing back-lined grout material has low slurry strength, large shrinkage, poor stability, easy to sink, and coarse particles, resulting in poor bonding performance of plugged pipes and materials, resulting in waterproofing and sulfate corrosion resistance. The performance is insufficient and it is difficult to effectively fill the lining wall gap.

Method used

High-strength non-shrinkable lining back-sorbing material is used to replace cement by using a large amount of slag powder, and excite it through alkali, combined with permeable crystalline waterproofing materials and plastic expansion agents to form an inner screen waterproof layer, enhancing impermeability and sulfate corrosion resistance Performance, reduce cement usage and reduce environmental pollution.

Benefits of technology

The high strength, durability and low cost of the grouting material are achieved, and the lining wall gaps are filled, and the excellent anti-seepage and sulfate corrosion resistance is provided, which reduces the expansion rate and enhances the compactness and structural strength of the concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968116600000071
    Figure BDA0004968116600000071
Patent Text Reader

Abstract

The invention discloses a high-strength shrinkage-free lining wall post-grouting material for a submarine mining method tunnel. The high-strength shrinkage-free lining wall post-grouting material comprises the following raw materials: cement, slag powder, lime, an alkali-activated material, sand, a high-efficiency water reducing agent, a defoaming agent, an expanding agent, a plastic expanding agent, cellulose and a capillary crystalline waterproof material. According to the invention, cement is replaced by slag powder with a large mixing amount, and the use amount of the cement is reduced through alkali excitation, so that not only is the strength of the grouting material ensured, but also the durability of the grouting material is enhanced, the environmental pollution is reduced, the cost is low, and the mortar has excellent sulfate corrosion resistance and corrosion resistance grade K150, and can better adapt to the subsea tunnel environment; after the capillary crystalline waterproof material and free alkali in the concrete are subjected to condensation reaction, branch-tendril-shaped fine particle crystals are formed, capillary pores and fine cracks of the concrete are sealed, an internal screen waterproof protection layer is formed, the compactness of the concrete is enhanced, and a plastic expanding agent is adopted to expand before slurry hardening, so that gaps are effectively filled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a grouting material for tunnel construction by mining method, and in particular to a high-strength non-shrinkage lining wall post-grouting material for submarine mining method tunnel. Background Art

[0002] When using the mining method to construct tunnels on the seabed or riverbed, we often encounter soft strata such as faults and broken zones, where fissure water is well developed and the water pressure is high. This places high demands on the waterproof performance of the mining method tunnel lining structure, and also places higher demands on the grouting materials behind the tunnel lining wall. During tunnel lining construction, if the pre-laid waterproof board is squeezed and cracked, the lining concrete structure needs to have excellent waterproof performance. Grouting behind the lining wall is an important measure to effectively fill the concrete voids and enhance the overall waterproof effect of the lining. At present, there are problems with the grouting materials behind the lining wall. First, the slurry strength is low, mostly M20 or M30, which is very different from the strength and elastic modulus of the lining concrete, and the deformation is inconsistent; second, the slurry is made of cement-based materials, which shrinks greatly after hardening. For some larger voids, the slurry shrinks after grouting, and there are still gaps, which makes it impossible for the waterproof board and the lining structure to fit closely, and water bags are easily formed in the voided parts; third, the slurry has poor stability, is easy to sink to the bottom and segregate, and is not conducive to construction; fourth, the coarse particles in the slurry are large in size, which is easy to block the pipes during grouting and makes construction difficult; fifth, the bonding performance between the grouting material and concrete is poor, and the elastic modulus of the two materials is very different, which is easy to produce an obvious stratified interface, and the stratified surface often becomes the weak layer of the lining structure.

[0003] Therefore, in the construction of submarine tunnels, it is necessary to pay attention to the problem of voids behind the lining and be able to fill the gaps behind the lining wall in time. At the same time, it is also necessary to have high impermeability and resistance to sulfate erosion. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a high-strength, non-shrinkage lining wall back-grouting material for submarine mining tunnels, which can fill the gaps behind the lining wall in time and also needs to have high impermeability and sulfate corrosion resistance.

[0005] The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnels of the present invention comprises the following components by weight: 20-30 parts of cement, 70-80 parts of slag powder, 30-40 parts of lime, 1-6 parts of alkali-activated material, 70-100 parts of sand, 0.1-1 parts of high-efficiency water reducing agent, 0.1-0.3 parts of defoaming agent, 0.1-0.5 parts of expansion agent, 0.01-0.1 parts of plastic expansion agent, 0.02-0.08 parts of cellulose, and 2-6 parts of permeable crystalline waterproof material;

[0006] Further, the raw materials include the following components by weight: 25 parts of cement, 75 parts of slag powder, 35 parts of lime, 4 parts of alkali-activated material, 90 parts of sand, 0.5 parts of high-efficiency water reducing agent, 0.2 parts of defoaming agent, 0.3 parts of expansion agent, 0.05 parts of plastic expansion agent, 0.05 parts of cellulose, and 4 parts of permeable crystalline waterproof material;

[0007] Further, the alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide;

[0008] Further, in terms of mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2;

[0009] Furthermore, the cement is sulphoaluminate cement or ferroaluminate cement, and the sand is dried machine-made sand with a particle size of 0.075-5 mm;

[0010] Further, the particle size of the sand is 2 mm;

[0011] Furthermore, the defoaming agent is a polyether-modified silicone defoaming agent; and the penetrating crystalline waterproof material is a cement-based penetrating crystalline waterproof material.

[0012] Beneficial effects of the present invention: The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnels of the present invention uses a large amount of slag powder to replace cement and is activated by alkali to reduce the amount of cement, which not only ensures the strength of the grouting material, the later strength of the grouting material mainly comes from the slag powder, but also enhances the durability of the grouting material, reduces environmental pollution, and has a low cost. The use of a large amount of mineral admixtures also enables the mortar to have excellent sulfate corrosion resistance, with a corrosion resistance grade of K150, which is better adapted to the submarine tunnel environment; after the penetration crystallization waterproof material and the free alkali in the concrete undergo condensation reaction, dendrite-like fine particle crystals are formed, the capillary pores and fine cracks of the concrete are closed, and an internal screen waterproof protective layer is formed to enhance the density of the concrete; a plastic expansion agent is used to expand the slurry before hardening to effectively fill the gaps, and the expansion rate after hardening is less than 0.2%; no expansion damage will be caused to the lining concrete structure. The high-strength non-shrinkage lining wall back grouting material for submarine mining tunnels of the present invention can timely fill the gaps behind the lining wall, and at the same time, it is also required to have high anti-seepage performance and anti-sulfate corrosion performance. Ordinary mortar has poor resistance to chloride ion penetration and poor resistance to salt crystallization destruction, while the chloride ion diffusion coefficient of the grouting material of the present invention can be reduced to 3×10 -12 m 2 / s, the elastic modulus of the grouting material after hardening can reach 33GPa, which is close to the elastic modulus of concrete. DETAILED DESCRIPTION

[0013] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0014] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0015] The high-strength non-shrinkage lining wall rear grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 20-30 parts of cement, 70-80 parts of slag powder, 30-40 parts of lime, 1-6 parts of alkali-activated material, 70-100 parts of sand, 0.1-1 parts of high-efficiency water reducing agent, 0.1-0.3 parts of defoaming agent, 0.1-0.5 parts of expansion agent, 0.01-0.1 parts of plastic expansion agent, 0.02-0.08 parts of cellulose, and 2-6 parts of permeable crystalline waterproof material. The use of a large amount of slag powder to replace cement and alkali activation can reduce the amount of cement, which not only ensures the strength of the grouting material, the later strength of the grouting material mainly comes from the slag powder, but also enhances the durability of the grouting material, reduces environmental pollution, and has a low cost. The use of a large amount of mineral admixtures also enables the mortar to have excellent resistance to sulfate erosion and better adapt to the submarine tunnel environment. It is preferred to use sulphoaluminate cement or ferroaluminate cement. Under normal hardening conditions, aluminate cement has a strong resistance to sulfate corrosion because the cement stone does not contain tricalcium aluminate and calcium hydroxide and has a large density. This series of cement has high early strength, good frost resistance, corrosion resistance and wear resistance. Therefore, in a sulfate environment, the strength of the grouting material consolidation body will not be affected, and it has an excellent effect of resisting sulfate erosion. Lime is used to increase the viscosity and thixotropy of the slurry, so that the slurry is still easy to pump and construct when the consistency is small. At the same time, lime is an air-hardening material that slowly hardens in a closed stratum, allowing the slurry to maintain good construction performance for a long time in the early stage, and gradually hardens in the later stage, further improving the strength and density of the consolidation body. The penetrating crystallization waterproof material is powdery and is an alkali-activated chemical penetrating concrete waterproofing agent. After condensation reaction with the free alkali in the concrete, it forms dendrite-like fine particle crystals, which close the capillaries and fine cracks of the concrete, forming an internal screen waterproof protective layer, and enhancing the density of the concrete. It is preferred to use cement-based permeable crystal waterproof coating, whose main components are silicate cement, selected quartz sand, special active chemical substances, etc. It is a gray powder material. The waterproof mechanism is to use water as a carrier, through the guidance of water, with the help of strong permeability, to transmit and fill in the micropores and capillaries of concrete, and to produce physical and chemical reactions to form water-insoluble dendrites and crystals. The crystals are combined with the concrete structure to form a closed waterproof layer as a whole, blocking water flow and other liquid erosion from any direction. The purpose of permanent waterproofing and chemical corrosion resistance is achieved, and at the same time, it plays a role in protecting steel bars and enhancing the strength of concrete structures. The main function of the defoamer is to control the foam in the mortar and improve the performance and quality of the mortar. The defoamer helps to reduce the surface tension in the mortar, so that air and other gases are quickly released from the mortar, thereby reducing bubbles and pores in the mortar. This helps to improve the density and strength of the mortar and make the mortar more uniform and viscous. In addition, the mortar defoamer can also improve the fluidity and plasticity of the mortar.Plastic expansion agent is made of bauxite mineral as the main material. It is sintered at 1700℃ in a nitrogen atmosphere in the presence of carbon and calcium oxide, and then ground into a yellow powder after surface treatment. Expansion principle and advantages: During the cement hydration process, the surface-treated plastic expansion agent has a certain hydrolysis resistance. It reacts slowly with water under alkaline conditions to produce gas, which can make the cement mixture expand before solidification. This expansion is caused by uniformly and densely distributed fine bubbles containing nitrogen, acetylene and other mixed gases, which does not corrode or damage concrete steel bars. The expansion agent does not shrink the volume of the slurry when it solidifies, and has a micro-expansion effect, so that the slurry fully fills the gaps behind the wall. The expansion agent generally uses calcium sulfoaluminate: including alunite expansion agent, CSA expansion agent, U-type expansion agent, etc. The main components are anhydrous calcium sulfoaluminate, alunite, gypsum, etc., or calcium oxide expansion agents are used. High-efficiency water reducers are commonly used water reducers for grouting materials, including naphthalene-based water reducers, melamine-based and modified melamine-based water reducers, aminosulfonate-based water reducers, aliphatic water reducers, anthracene-based water reducers and washing oil-based water reducers, all of which can achieve the purpose of the present invention.

[0016] A preferred embodiment has raw materials comprising the following components by weight: 25 parts of cement, 75 parts of slag powder, 35 parts of lime, 4 parts of alkali-activated material, 90 parts of sand, 0.5 parts of high-efficiency water reducing agent, 0.2 parts of defoaming agent, 0.3 parts of expansion agent, 0.05 parts of plastic expansion agent, 0.05 parts of cellulose, and 4 parts of penetrating crystalline waterproof material; the effect of this embodiment is significantly better than that of other embodiments.

[0017] In this embodiment, the alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; in terms of mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2; through alkali activation, the amount of cement is reduced, and a large amount of slag powder is used, which not only ensures the strength of the grouting material, but also enhances the durability of the grouting material.

[0018] In this embodiment, the sand is dried machine-made sand with a particle size of 0.075-5 mm; preferably, the particle size is 2 mm;

[0019] In this embodiment, the defoamer is a polyether-modified silicone defoamer; and the penetrating crystallization type waterproof material is a cement-based penetrating crystallization type waterproof material. The polyether-modified silicone defoamer is a polyether-siloxane copolymer (referred to as silicone ether copolymer) obtained by introducing a polyether segment into a siloxane molecule. The polyether-modified silicone defoamer is a new type of high-efficiency defoamer that organically combines the advantages of both. It is a defoamer that selects polyether with strong anti-foaming ability and dimethyl silicone oil with strong hydrophobicity and rapid bubble breaking as the main ingredients, and is matched with an emulsifier, stabilizer and other ingredients that can organically combine silicone oil and polyether. It has the characteristics of low surface tension, rapid defoaming, long anti-foaming time, low cost, small dosage, and wide application.

[0020] The method for preparing the high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment is to mix and stir the above raw materials evenly according to a conventional grouting material mixing method and then carry out construction.

[0021] Embodiment 1

[0022] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 20 parts of cement, 70 parts of slag powder, 30 parts of lime, 1 part of alkali-activated material, 70 parts of sand, 0.1 part of high-efficiency water reducer (naphthalene-based water reducer), 0.1 part of polyether-modified organic silicon defoamer, 0.1-0.5 part of expansion agent (alumite expansion agent), 0.01 part of plastic expansion agent, 0.02 part of cellulose, and 2 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; by mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0023] Embodiment 2

[0024] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 30 parts of cement, 80 parts of slag powder, 40 parts of lime, 6 parts of alkali-activated materials, 100 parts of sand, 1 part of high-efficiency water reducer (melamine-based water reducer), 0.3 parts of polyether-modified silicone defoamer, 0.5 parts of expansion agent (CSA expansion agent), 0.1 parts of plastic expansion agent, 0.08 parts of cellulose, and 6 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; by mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0025] Embodiment 3

[0026] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 20 parts of cement, 80 parts of slag powder, 30 parts of lime, 6 parts of alkali-activated materials, 70 parts of sand, 0.1 parts of high-efficiency water reducer (naphthalene-based water reducer), 0.3 parts of polyether-modified silicone defoamer, 0.1-0.5 parts of expansion agent (alumite expansion agent), 0.01 parts of plastic expansion agent, 0.08 parts of cellulose, and 2 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; by mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0027] Embodiment 4

[0028] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 28 parts of cement, 75 parts of slag powder, 38 parts of lime, 2 parts of alkali-activated material, 80 parts of sand, 0.7 parts of high-efficiency water reducer (modified melamine-based water reducer), 0.25 parts of polyether-modified silicone defoamer, 0.15 parts of expansion agent (alumite expansion agent), 0.08 parts of plastic expansion agent, 0.03 parts of cellulose, and 3 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; by mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0029] Embodiment 5

[0030] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 24 parts of cement, 75 parts of slag powder, 33 parts of lime, 3 parts of alkali-activated material, 90 parts of sand, 0.7 parts of high-efficiency water reducer (aminosulfonate water reducer), 0.2 parts of polyether-modified silicone defoamer, 0.4 parts of expansion agent (alumite expansion agent), 0.05 parts of plastic expansion agent, 0.04 parts of cellulose, and 5 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; by mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0031] Embodiment 6

[0032] The high-strength, non-shrinkage lining wall post-grouting material for submarine mining tunnels of this embodiment comprises the following components by weight: 25 parts of cement, 75 parts of slag powder, 35 parts of lime, 4 parts of alkali-activated material, 90 parts of sand, 0.5 parts of high-efficiency water reducer (aliphatic water reducer), 0.2 parts of polyether-modified silicone defoamer, 0.3 parts of expansion agent (alum stone expansion agent), 0.05 parts of plastic expansion agent, 0.05 parts of cellulose, and 4 parts of cement-based penetrating crystalline waterproof material. The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide; in terms of mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:2.

[0033] The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnels in Example 1 was subjected to performance tests according to conventional methods in the prior art. The test results are as follows:

[0034]

[0035] It can be seen that the high-strength non-shrinkage lining wall back-injection grouting material for submarine mining tunnels of the present invention has a fluidity of 380mm-410mm, a water seepage rate of 0%, a 28d compressive strength greater than 50MPa, a micro-expansion of 0.3-2.0%, a permeability greater than 1.5MPa, and a strong bonding with lining concrete. The effect of the high-strength non-shrinkage lining wall back-injection grouting material for submarine mining tunnels of the above-mentioned Examples 2-6 is significantly better than that of Example 1.

[0036] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnels. Features: The raw materials include the following components by weight: 20-30 parts of cement, 70-80 parts of slag powder, 30-40 parts of lime, 1-6 parts of alkali-activated material, 70-100 parts of sand, 0.1-1 parts of high-efficiency water reducing agent, 0.1-0.3 parts of defoaming agent, 0.1-0.5 parts of expansion agent, 0.01-0.1 parts of plastic expansion agent, 0.02-0.08 parts of cellulose, and 2-6 parts of penetrating crystalline waterproof material.

2. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 1, Features: The raw materials include the following components by weight: 25 parts of cement, 75 parts of slag powder, 35 parts of lime, 4 parts of alkali-activated material, 90 parts of sand, 0.5 parts of high-efficiency water reducing agent, 0.2 parts of defoaming agent, 0.3 parts of expansion agent, 0.05 parts of plastic expansion agent, 0.05 parts of cellulose, and 4 parts of penetrating crystalline waterproof material.

3. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 1, Features: The alkali-activated material is a mixture of sodium silicate, calcium sulfate and calcium oxide.

4. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 3, Features: By mass ratio, sodium silicate: calcium sulfate: calcium oxide = 1:3:

2.

5. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 1, Features: The cement is sulphoaluminate cement or ferroaluminate cement, and the sand is dried machine-made sand with a particle size of 0.075-5 mm.

6. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 5, Features: The sand particle size is 2 mm.

7. The high-strength non-shrinkage lining wall post-grouting material for submarine mining tunnel according to claim 1, Features: The defoaming agent is a polyether modified silicone defoaming agent; the penetrating crystalline waterproof material is a cement-based penetrating crystalline waterproof material.

Citation Information

Patent Citations

  • Micro expansion grouting material for tunnel lining filling

    CN107686300A

  • Micro-expansion grouting material for grouting tunnel lining vault with mold

    CN108558330A

  • High-strength self-stress coal mine bottom plate grouting reinforcement material and preparation method thereof

    CN111960781A

  • Early-strength capillary crystalline grouting material for filling lining cavity of operating tunnel and preparation method of grouting slurry

    CN116003060A

Cited By

  • Alkali-salt synergy-based alkali-activated tunnel lining repair material and preparation method thereof

    CN120247523A

  • High-damping strong-toughness tunnel lining wall back filling material as well as preparation method and application of high-damping strong-toughness tunnel lining wall back filling material

    CN122380790A