InGaN (indium gallium tin oxide) sputtering target material and preparation method thereof
By preparing IGTO sputtering targets with high density and fine grains, the problems of density and grain size control of IGTO targets were solved, sputtering stability and thin film properties were improved, and target performance with high density and low resistivity was achieved.
Patent Information
- Application Number
- CN202411038508.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing technologies struggle to improve the density of indium gallium tin oxide (IGTO) targets and control their grain size, which affects sputtering stability and thin film properties.
IGTO slurry was prepared by stoichiometric mixing of indium oxide, gallium oxide, tin oxide, deionized water, dispersant and binder. High-density fine-grained IGTO sputtering targets were prepared by pressure casting and debinding-pressureless sintering integrated technology.
High density and uniform microstructure of IGTO sputtering targets were achieved, with a relative density of 98.2-99.8% and a volume resistivity of 0.2-0.6 mΩ·cm, which are significantly better than existing methods.
Smart Images

Figure CN118955093A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic device materials, and in particular to an indium gallium tin oxide sputtering target material and a preparation method thereof. Background Art
[0002] Transparent conductive oxide thin films (TCO) are a class of special functional materials with good optical properties and conductivity. They are widely used in electronic screens, touch screen panels, light-emitting diodes (LEDs) and solar cells. This type of material is easy to produce and can be prepared using techniques such as chemical vapor deposition, magnetron sputtering and spray pyrolysis. The most commonly used TCOs are tin-doped indium oxide (indium tin oxide or ITO) and indium gallium zinc oxide (IGZO) systems.
[0003] Compared with tin-doped indium oxide (ITO) and aluminum-doped zinc oxide (AZO) material systems, indium gallium tin oxide (IGTO) films prepared from indium gallium tin oxide material systems have higher carrier mobility. Therefore, their excellent optoelectronic properties can be further improved without increasing the carrier concentration (maintaining high transmittance).
[0004] Indium gallium tin oxide (IGTO) film can also be used as a channel layer material in thin film transistor (TFT) devices. Compared with indium gallium zinc oxide (IGZO) film, In indium gallium tin oxide (IGTO) film has a higher In 3+ and Sn 4+ The ions have the same electronic structure, so that Sn can enhance the percolation conduction path in the oxide film through the extensive overlap of adjacent large 5s orbitals, thus enabling higher field-effect mobility to be obtained at lower annealing temperatures.
[0005] At present, the preparation of indium gallium tin oxide (IGTO) thin films mainly adopts magnetron sputtering, and the density and grain size of the sputtering target are important factors affecting the sputtering stability and film properties.
[0006] Therefore, how to improve the density of IGTO target and control its grain size has become the primary technical problem to be solved in this field. Summary of the invention
[0007] The object of the present invention is to provide a low resistivity indium gallium tin oxide sputtering target and a preparation method thereof to solve the problems mentioned in the background technology. The indium gallium tin oxide (IGTO) sputtering target prepared by the preparation method proposed in the present invention has high-density fine grains.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] A method for preparing a low-resistivity indium gallium tin oxide sputtering target comprises the following steps:
[0010] S1. Mixing indium oxide, gallium oxide, tin oxide, deionized water, a dispersant and a binder according to a stoichiometric ratio to obtain an indium gallium tin oxide slurry;
[0011] S2, performing pressure injection molding on the indium gallium tin oxide (IGTO) slurry obtained in S1, and obtaining an indium gallium tin oxide (IGTO) sputtering target blank after drying;
[0012] S3. The indium gallium tin oxide (IGTO) sputtering target blank obtained in S2 is processed by using a degreasing-pressureless sintering integrated technology to obtain an indium gallium tin oxide (IGTO) sputtering target.
[0013] Preferably, the number of indium atoms in the indium gallium tin oxide (IGTO) slurry obtained in S1 is 70% of the total number of indium, gallium and tin atoms;
[0014] Preferably, the number of gallium atoms in the indium gallium tin oxide (IGTO) slurry obtained in S1 is 10-20% of the total number of indium, gallium and tin atoms.
[0015] Preferably, the mass of the dispersant in S1 is 0.5-1.8% of the total mass of indium oxide, gallium oxide and tin oxide.
[0016] Preferably, the mass of the binder in S1 is 0.3-2.5% of the total mass of indium oxide, gallium oxide and tin oxide.
[0017] Preferably, the solid content of the indium gallium tin oxide (IGTO) slurry obtained in S1 is greater than 75%, and the viscosity is less than 100 mPa·s.
[0018] Preferably, it is characterized in that the pressure grouting forming in S2 specifically includes the following contents:
[0019] Before pressure grouting, the indium gallium tin oxide (IGTO) slurry is subjected to vacuum degassing treatment; the mold material used in the pressure grouting is gypsum; and the pressure of the pressure grouting is 0.1-0.4 MPa.
[0020] Preferably, the drying operation in S2 is performed in a constant temperature and humidity chamber, specifically including the following contents:
[0021] The oven temperature is 30-35°C; the ambient humidity is 50-60%RH; the drying time is 48-72h; and the quality of the sputtering target blank is kept constant.
[0022] Preferably, the temperature of the degreasing treatment in S3 is 650-800° C., and the holding time of the degreasing treatment is 12-24 hours.
[0023] Preferably, the pressureless sintering process in S3 specifically includes the following contents:
[0024] The sintering atmosphere is oxygen; the heating rate is 3°C / min; the holding temperature is 1400-1600°C; and the cooling rate is 1-5°C / min.
[0025] Indium gallium tin oxide (IGTO) sputtering target prepared by the above preparation method.
[0026] Compared with the prior art, the present invention provides a method and system for generating a numerical reactor unitized efficient integrated grid, which has the following beneficial effects:
[0027] The present invention provides an indium gallium tin oxide sputtering target and a preparation method thereof. Indium oxide powder, gallium oxide powder and tin oxide powder are added to a ball mill according to a certain indium gallium tin atomic ratio (70:15:15, 70:10:20, 70:20:10), and deionized water, a dispersant and a binder are added. A high-energy ball milling technology is used to prepare a high-solid content and low-viscosity IGTO slurry; a pressure injection molding technology is used to prepare a high-density IGTO sputtering target blank; a degreasing process is used to remove the dispersant and the binder, and combined with pressureless flow atmosphere sintering, the target material has a uniform structure and high density. The experimental results of the embodiment show that the relative density of the indium gallium tin oxide sputtering target prepared by the preparation method provided by the present invention is 98.2-99.8%, and the performance is significantly better than the existing preparation methods on the market. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is an overall flow chart of a method for preparing an indium gallium tin oxide sputtering target material proposed by the present invention;
[0029] Figure 2 The phase composition and microstructure diagram of the IGTO sputtering target prepared in Example 1 of the present invention;
[0030] Figure 3 The phase composition and microstructure diagram of the IGTO sputtering target prepared in Example 2 of the present invention;
[0031] Figure 4 This is the phase composition and microstructure diagram of the IGTO sputtering target prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0033] The present invention provides an indium gallium tin oxide sputtering target and a preparation method thereof, comprising the following steps:
[0034] (1) mixing indium oxide, gallium oxide, tin oxide, deionized water, a dispersant and a binder according to a stoichiometric ratio to obtain an IGTO slurry;
[0035] (2) subjecting the IGTO slurry obtained in step (1) to pressure casting, and obtaining an IGTO sputtering target blank after drying;
[0036] (3) The IGTO sputtering target blank obtained in step (2) is subjected to degreasing treatment and pressureless flow atmosphere sintering in sequence to obtain an indium gallium tin oxide sputtering target.
[0037] Unless otherwise specified, the present invention has no particular limitation on the sources of the components, and commercially available products known to those skilled in the art may be used.
[0038] The present invention mixes indium oxide, gallium oxide, tin oxide, deionized water, a dispersant and a binder according to a stoichiometric ratio to obtain an IGTO slurry;
[0039] In the present invention, the indium oxide, gallium oxide and tin oxide are preferably nanopowders: the particle sizes of the indium oxide, gallium oxide and tin oxide are preferably 100 to 300 nm, more preferably 150 to 250 nm.
[0040] The present invention has no special limitation on the mixing operation of the indium oxide, gallium oxide and tin oxide, and the two can be uniformly mixed by using a powder mixing technical solution well known to those skilled in the art. In the present invention, the mixing of the indium oxide, gallium oxide and tin oxide is preferably carried out in a high-efficiency mixer, a jet mill or a ball mill.
[0041] The invention mixes indium oxide, gallium oxide, tin oxide, deionized water, a dispersant and a binder to obtain IGTO slurry.
[0042] In the present invention, the dispersant is preferably ammonium polyacrylate or a polycarboxylic acid dispersant. In the present invention, the mass of the dispersant is preferably 0.8-1.6% of the total mass of indium oxide, gallium oxide and tin oxide, more preferably 1.0-1.4%, and most preferably 1.2%. The present invention controls the mass of the dispersant within the above range, which can ensure that the oxide powder is fully and evenly dispersed in the slurry, which is conducive to obtaining an IGTO sputtering target with uniform phase distribution.
[0043] In the present invention, the binder is preferably polyvinyl alcohol or gum arabic. In the present invention, the mass of the binder is preferably 0.3-1.0% of the total mass of indium oxide, gallium oxide and tin oxide, more preferably 0.4-0.9%, and most preferably 0.5-0.8%. The present invention controls the mass of the binder within the above range, which can ensure that the slurry has a suitable viscosity, and at the same time, the obtained IGTO sputtering target blank has a suitable density, thereby improving the density of the target material.
[0044] In the present invention, the mass of the water is preferably 16-20% of the total mass of indium oxide, gallium oxide and tin oxide, more preferably 17-19%, and most preferably 18%. The present invention controls the amount of water within the above range, which can ensure that the slurry has a suitable solid content, promote the oxide powder to be fully and evenly dispersed in the slurry, and is conducive to obtaining an IGTO sputtering target with uniform phase distribution.
[0045] In the present invention, the solid content of the IGTO slurry is preferably greater than 75%, more preferably less than 80%. In the present invention, the viscosity of the IGTO slurry is preferably less than 100 mPa·s, more preferably greater than 50 mPa·s. The present invention controls the viscosity and solid content of the IGTO slurry within the above range, which is conducive to the full and uniform dispersion of the oxide powder in the slurry, while making the slurry have a suitable viscosity, which is conducive to obtaining an IGTO sputtering target with uniform phase distribution and high density.
[0046] In the present invention, the mixing of indium oxide, gallium oxide, tin oxide, deionized water, dispersant and binder is preferably ball milled. The present invention can evenly mix indium oxide, gallium oxide and tin oxide through ball milling, which is conducive to obtaining an IGTO sputtering target with uniform phase distribution.
[0047] In the present invention, the addition of the dispersant will cause the pH value of the slurry to change. In the present invention, the Zeta potential value of the slurry as the pH changes is preferably detected by a nano-particle size potentiometer to ensure that the slurry is in an optimal dispersion state.
[0048] After obtaining the IGTO slurry, the present invention performs pressure injection molding on the IGTO slurry to obtain an IGTO sputtering target blank.
[0049] In the present invention, the pressure of the pressure grouting molding is preferably 0.1-0.4 MPa. In the present invention, the mold used for the pressure grouting molding is preferably made of gypsum. The pressure grouting molding method used in the present invention can prepare a target blank with a larger size, and the operation is simple and cost-saving.
[0050] The present invention preferably performs vacuum degassing treatment on the IGTO slurry before pressure injection molding; the vacuum pressure of the vacuum degassing treatment is preferably lower than 0.1 Pa. In the present invention, the vacuum degassing treatment can remove gas in the slurry, which is conducive to obtaining a high-density IGTO sputtering target blank.
[0051] After the pressure casting is completed, the present invention preferably dries the product obtained by the pressure casting to obtain an IGTO sputtering target blank. The present invention can remove residual moisture by drying.
[0052] In the present invention, the drying temperature is preferably 30-35° C.; the low-temperature drying environment humidity is preferably 50-60% RH; and the low-temperature drying time is preferably 48-72 hours.
[0053] In the present invention, the drying is preferably performed in a constant temperature and humidity chamber.
[0054] In the present invention, the relative density of the IGTO sputtering target green body is preferably 60% or more.
[0055] After obtaining the IGTO sputtering target blank, the present invention sequentially performs degreasing treatment and pressureless flow atmosphere sintering on the IGTO sputtering target blank to obtain an indium gallium tin oxide sputtering target.
[0056] In the present invention, the temperature of the degreasing treatment is preferably 650-800°C; the holding time of the degreasing treatment is preferably 12-24h; in the present invention, the rate of heating to the degreasing treatment temperature is preferably 0.5-1.5°C / min. The present invention can remove the binder and dispersant in the IGTO blank through the degreasing treatment.
[0057] In the present invention, after the degreasing treatment is completed, the pressureless flow atmosphere sintering is directly performed without cooling.
[0058] In the present invention, the pressureless flowing atmosphere sintering preferably includes:
[0059] The sintering atmosphere is preferably oxygen; the heating rate is preferably 6°C / min; the holding temperature is preferably 1400-1600°C, more preferably 1450-1550°C; and the cooling method is preferably furnace cooling.
[0060] After the pressureless flowing atmosphere sintering is completed, the indium gallium tin oxide sputtering target is obtained.
[0061] The present invention adopts the pressure grouting forming method to prepare target material blanks with larger sizes, and the operation is simple and cost-saving.
[0062] The present invention provides an indium gallium tin oxide sputtering target material prepared by the preparation method described in the above technical solution. The indium gallium tin oxide sputtering target material provided by the present invention has uniform structure and high density.
[0063] In the present invention, the relative density of the indium gallium tin oxide sputtering target is 98.2-99.8%, and the volume resistivity is 0.2-0.6 mΩ·cm.
[0064] Based on the above content, the specific example content is as follows.
[0065] Example 1
[0066] Nano-scale indium oxide powder, gallium oxide powder and tin oxide powder were weighed according to the atomic ratio of indium: gallium: tin = 70:15:15 at.%, with a total mass of 800 g of powder, including 580.84 g of indium oxide powder, 84.03 g of gallium oxide powder and 135.13 g of tin oxide powder. 200 g of deionized water accounting for 25% of the total mass of the powder and 1.2% of ammonium polyacrylate (NH4OH) accounting for 1% of the total mass of the powder were added to the mixed powder. 4 PAA) 9.6g, polyvinyl alcohol (NH 4 PAA) 6.4 g, to obtain an IGTO slurry with a solid content of 79.06% and a viscosity of 90 mPa·s;
[0067] The prepared slurry is dispersed by ball milling, the ball mill speed is 300rpm, the time is 72h, the IGTO slurry after sand milling is vacuumed and defoamed to avoid the generation of large bubbles in the slurry, and then the IGTO sputtering target blank is obtained by pressure grouting forming process, wherein the grouting pressure is 0.3MPa, the pressure holding time is 3h, the sputtering target blank is taken out and placed in a constant temperature and humidity box for drying, the temperature in the oven is 35°C, the humidity is 60%RH, and it is dried for 48h until the mass of the sputtering target blank remains constant, and finally an IGTO sputtering target blank with a relative density of 60% is obtained;
[0068] The IGTO sputtering target blank was degreased at a heating rate of 1°C / min, a degreasing temperature of 700°C, and a holding time of 18h. The degreased IGTO sputtering target blank directly entered the sintering process and was sintered in a pressureless flowing atmosphere at a heating rate of 6°C / min to 1500°C and held for 10h. After the furnace heating was completed, the target sintered body was cooled with the furnace to obtain the phase In 2 O 3 and Ga 2 In 6 Sn 2 O 16 Uniformly distributed IGTO sputtering target, phase composition and microstructure such as Figure 1 shown.
[0069] According to the Archimedean principle and a four-probe instrument, the density and resistivity of the IGTO sputtering target prepared in this embodiment were tested respectively, and the relative density was 99.1% and the volume resistivity was 0.5 mΩ·cm.
[0070] Example 2
[0071] Nano-scale indium oxide powder, gallium oxide powder and tin oxide powder were weighed according to the atomic ratio of indium: gallium: tin = 70:10:20 at.%, with a total mass of 800 g of the powder, including 568.73 g of indium oxide powder, 54.85 g of gallium oxide powder and 176.41 g of tin oxide powder. 200 g of deionized water accounting for 25% of the total mass of the powder, 9.6 g of ammonium polyacrylate (NH4PAA) accounting for 1.2% of the total mass of the powder, and 6.4 g of polyvinyl alcohol (NH4PAA) accounting for 0.8% of the total mass of the powder were added to the mixed powder to obtain an IGTO slurry with a solid content of 79.06% and a viscosity of 90 mPa·s;
[0072] The prepared slurry is dispersed by ball milling, the ball mill speed is 300rpm, the time is 72h, the IGTO slurry after sand milling is vacuumed and defoamed to avoid the generation of large bubbles in the slurry, and then the IGTO sputtering target blank is obtained by pressure grouting forming process, wherein the grouting pressure is 0.3MPa, the pressure holding time is 3h, the sputtering target blank is taken out and placed in a constant temperature and humidity box for drying, the temperature in the oven is 35°C, the humidity is 60%RH, and it is dried for 48h until the mass of the sputtering target blank remains constant, and finally an IGTO sputtering target blank with a relative density of 60% is obtained;
[0073] The IGTO sputtering target blank was degreased at a heating rate of 1°C / min, a degreasing temperature of 700°C, and a holding time of 18h. The degreased IGTO sputtering target blank directly entered the sintering process and was sintered in a pressureless flowing atmosphere at a heating rate of 6°C / min to 1500°C and held for 10h. After the furnace heating was completed, the target sintered body was cooled with the furnace to obtain the phase In 2 O 3 and Ga 1.6 In 6.4 Sn 2 O 16 Uniformly distributed IGTO sputtering target, phase composition and microstructure such as Figure 2 shown.
[0074] According to the Archimedean principle and a four-probe instrument, the density and resistivity of the IGTO sputtering target prepared in this embodiment were tested respectively, and the relative density was 98.2% and the volume resistivity was 0.4 mΩ·cm.
[0075] Example 3
[0076] Nano-scale indium oxide powder, gallium oxide powder and tin oxide powder were weighed according to the atomic ratio of indium: gallium: tin = 70:20:10 at.%, with a total mass of 800 g of powder, including 593.48 g of indium oxide powder, 114.48 g of gallium oxide powder and 92.04 g of tin oxide powder. 200 g of deionized water accounting for 25% of the total mass of the powder and 1.2% of ammonium polyacrylate (NH4OH) accounting for 1% of the total mass of the powder were added to the mixed powder. 4 PAA) 9.6g, polyvinyl alcohol (NH 4 PAA) 6.4 g, to obtain an IGTO slurry with a solid content of 79.06% and a viscosity of 90 mPa·s;
[0077] The prepared slurry is dispersed by ball milling, the ball mill speed is 300rpm, the time is 72h, the IGTO slurry after sand milling is vacuumed and defoamed to avoid the generation of large bubbles in the slurry, and then the IGTO sputtering target blank is obtained by pressure grouting forming process, wherein the grouting pressure is 0.3MPa, the pressure holding time is 3h, the sputtering target blank is taken out and placed in a constant temperature and humidity box for drying, the temperature in the oven is 35°C, the humidity is 60%RH, and it is dried for 48h until the mass of the sputtering target blank remains constant, and finally an IGTO sputtering target blank with a relative density of 60% is obtained;
[0078] The IGTO sputtering target blank was degreased at a heating rate of 1°C / min, a degreasing temperature of 700°C, and a holding time of 18h. The degreased IGTO sputtering target blank directly entered the sintering process and was sintered in a pressureless flowing atmosphere at a heating rate of 6°C / min to 1500°C and held for 10h. After the furnace heating was completed, the target sintered body was cooled with the furnace to obtain the phase In 2 O 3 , Ga 1.6 In 6.4 Sn 2 O 16 and GaInO 3 Uniformly distributed IGTO sputtering target, phase composition and microstructure such as Figure 3 shown.
[0079] According to the Archimedean principle and a four-probe instrument, the density and resistivity of the IGTO sputtering target prepared in this embodiment were tested respectively, and the relative density was 99.8% and the volume resistivity was 0.4 mΩ·cm.
[0080] It can be seen from the above embodiments that the preparation method provided by the present invention is easy to operate, saves costs, and the prepared IGTO sputtering target has uniform structure, high density and low resistivity.
[0081] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a low resistivity indium gallium tin oxide sputtering target, characterized in that: The following steps are involved: S1. Mixing indium oxide, gallium oxide, tin oxide, deionized water, a dispersant and a binder according to a stoichiometric ratio to obtain an indium gallium tin oxide slurry; S2, performing pressure injection molding on the indium gallium tin oxide slurry obtained in S1, and obtaining an indium gallium tin oxide sputtering target blank after drying; S3. The indium gallium tin oxide sputtering target blank obtained in S2 is processed by a degreasing-pressureless sintering integrated technology to obtain an indium gallium tin oxide sputtering target.
2. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The number of indium atoms in the indium gallium tin oxide slurry obtained in S1 is 70% of the total number of indium, gallium and tin atoms; The number of gallium atoms in the indium gallium tin oxide slurry obtained in S1 is 10-20% of the total number of indium, gallium and tin atoms.
3. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The mass of the dispersant in S1 is 0.5-1.8% of the total mass of indium oxide, gallium oxide and tin oxide.
4. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The mass of the binder in S1 is 0.3-2.5% of the total mass of indium oxide, gallium oxide and tin oxide.
5. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The solid content of the indium gallium tin oxide slurry obtained in S1 is greater than 75%, and the viscosity is less than 100 mPa·s.
6. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The pressure grouting forming described in S2 specifically includes the following contents: Before pressure grouting, the indium gallium tin oxide slurry is subjected to vacuum degassing treatment; the mold material used in the pressure grouting is gypsum; and the pressure of the pressure grouting is 0.1-0.4 MPa.
7. The method for preparing an IGTO sputtering target according to claim 1, characterized in that: The drying operation in S2 is carried out in a constant temperature and humidity chamber, which specifically includes the following contents: The oven temperature is 30-35°C; the ambient humidity is 50-60%RH; the drying time is 48-72h; and the quality of the sputtering target blank is kept constant.
8. The method for preparing a low resistivity indium gallium tin oxide sputtering target according to claim 1, characterized in that: The temperature of the degreasing treatment in S3 is 650-800° C., and the holding time of the degreasing treatment is 12-24 hours.
9. The method for preparing a low resistivity InGaTnO sputtering target according to claim 1, characterized in that: The pressureless sintering process described in S3 specifically includes the following contents: The sintering atmosphere is oxygen; the heating rate is 3°C / min; the holding temperature is 1400-1600°C; and the cooling rate is 1-5°C / min.
10. An indium gallium tin oxide sputtering target prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
In-Ga-Sn oxide sinter, target, oxide semiconductor film, and semiconductor element
CN102770577A
Preparation method for low-scaffolding indium tin oxide target material
CN109369172A
Rare earth element doped indium tin gallium oxide target material and preparation method thereof
CN116813310A
Oxide indium tin sputtering target, transparent conductive film manufactured thereby and method for manufacturing transparent conductive film, and display device comprising same
KR1020140093048A
Cited By
MOS (Metal Oxide Semiconductor) target material, preparation method thereof and thin film transistor
CN119683970A
A MOS target, a preparation method thereof, and a thin film transistor
CN119683970B