Mineral powder reinforced polyurethane grouting material as well as preparation method and application thereof

By preparing ore powder-enhanced polyurethane grouting materials, the problems of insufficient UV aging resistance and low temperature stability of existing crack repair materials are solved, and the efficient, economical and long-term effects of asphalt pavement gap repair are achieved.

CN118955854APending Publication Date: 2024-11-15CHANGAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411257264.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing crack repair materials have shortcomings in their UV aging resistance, low temperature stability and durability, and cannot meet the actual needs of asphalt pavement gap repair.

Method used

Polyols, isocyanates, ore powder, curing agents and crosslinking agents are used to prepare ore powder-enhanced polyurethane grouting materials. The urethane grouting materials are formed through pretreatment and reprocessing, and the ore powder dosage is optimized to 30% to improve the mechanics of the material. Performance and thermal stability.

Benefits of technology

It significantly improves the UV aging resistance, low temperature stability and durability of polyurethane grouting materials, and reduces maintenance costs. The repaired specimens perform better than traditional in low-temperature splitting tensile strength, low-temperature bending performance and freeze-thaw cycle tests. Material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955854A_ABST
    Figure CN118955854A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of road materials, and relates to a mineral powder reinforced polyurethane grouting material and a preparation method and application thereof.The preparation method comprises the steps that S1, a polyurethane prepolymer is prepared, specifically, in the nitrogen atmosphere, polyol and isocyanate are adopted to prepare the polyurethane prepolymer; s2, preparing a mineral powder reinforced polyurethane grouting material: pretreating a polyurethane prepolymer, adding mineral powder, and uniformly mixing; and after secondary treatment, mixing with a curing agent and a cross-linking agent to obtain the urethane grouting material. The adding mass of the mineral powder is 10%-40% of the mass of the urethane grouting material. The mineral powder reinforced polyurethane grouting material prepared by the invention not only has excellent ultraviolet aging resistance, but also has better durability and low-temperature stability, and can be well used in asphalt pavement crack repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road materials and relates to a mineral powder reinforced polyurethane grouting material and a preparation method and application thereof. Background Art

[0002] During the use of asphalt pavement, due to the combined influence of multiple factors such as bad weather, complex traffic loads and poor construction quality, various diseases will inevitably occur. Among these diseases, cracks are the most common and serious form of damage, accounting for about 70% of the total number of diseases. The appearance of cracks not only indicates the destruction of the pavement structure, but also allows surface water and impurities to penetrate into the pavement; more seriously, when cracks penetrate the roadbed, they will weaken the stability of the roadbed, thereby reducing the bearing capacity of the pavement, and the structural diseases caused by them seriously restrict the service life of the asphalt pavement. Therefore, timely and effective repair of cracks is the key to ensuring the long-term service of asphalt pavement.

[0003] The Chinese patent document with reference publication number CN114988788A discloses a material for repairing potholes in asphalt pavement and a preparation method thereof. Although the material can be repaired, it mainly repairs potholes and cannot meet the requirements of repairing cracks in pavement. At present, there are some crack repair materials, such as emulsified asphalt and modified asphalt, etc. However, these repair materials have problems such as poor durability, insufficient adhesion, high cost, insufficient bearing capacity and complex construction process; in addition, some researchers use polyurethane materials with good adhesion properties, which can be firmly attached to the concrete surface to form an integrated structure. Although it can be used for crack repair, the amount of polyurethane materials used is large, the cost is high, and there are also shortcomings such as insufficient anti-ultraviolet aging performance, poor low-temperature stability and poor durability, which cannot meet the actual needs of asphalt pavement crack repair. Summary of the invention

[0004] In view of the technical problems that existing crack repair materials have insufficient anti-ultraviolet aging performance, poor low-temperature stability and poor durability, the present invention provides a mineral powder reinforced polyurethane grouting material and a preparation method and application thereof.

[0005] The invention adopts polyol, isocyanate, mineral powder, curing agent and cross-linking agent to prepare mineral powder reinforced polyurethane grouting material, which not only has excellent anti-ultraviolet aging performance, but also has good durability and low-temperature stability, and can be well used in the repair of asphalt pavement cracks.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a mineral powder reinforced polyurethane grouting material comprises the following steps:

[0008] S1. Preparation of polyurethane prepolymer

[0009] In a nitrogen atmosphere, a polyurethane prepolymer is prepared by using polyol and isocyanate;

[0010] S2. Preparation of mineral powder reinforced polyurethane grouting material

[0011] The polyurethane prepolymer of step S1 is pretreated, and then mineral powder is added and mixed evenly; after being treated again, it is mixed with a curing agent and a cross-linking agent to obtain an urethane grouting material; the mass of the added mineral powder is 10% to 40% of the mass of the urethane grouting material; the mass ratio of the curing agent to the polyurethane prepolymer is 14.5:100; and the molar ratio of the cross-linking agent to the polyurethane prepolymer is 1:1.

[0012] It is further defined that in step S2, the curing agent is an addition product of toluene diisocyanate and trimethylolpropane, 4,4'-diisocyanate diphenyl ester, or 2,4-diisocyanato-1,6-hexamethylene diisocyanate trimer; and the cross-linking agent is butanediol, glycerol or propylene glycol.

[0013] It is further defined that the pretreatment is a treatment at a temperature of 80°C to 90°C for 30 minutes to 50 minutes; and the secondary treatment is a treatment at a temperature of 80°C to 90°C for 15 minutes to 30 minutes.

[0014] It is further defined that in step S1, the preparation process of the polyurethane prepolymer is:

[0015] The polyol is vacuum dehydrated and cooled, then mixed with isocyanate, heated, fully reacted under a nitrogen atmosphere, and then vacuumed to obtain a polyurethane prepolymer.

[0016] In a further embodiment, the polyol is a polyether polyol, a polytetramethylene ether glycol or a polyester polyol.

[0017] It is further defined that the vacuum dehydration and cooling process is to carry out vacuum dehydration treatment at a temperature of 110°C to 130°C for 1h to 2h and then reduce the temperature to 65°C.

[0018] It is further defined that the heating temperature is 80°C to 85°C, the reaction is fully carried out for 1h to 2h, and the vacuum is drawn for 0.5h to 1h.

[0019] The mineral powder reinforced polyurethane grouting material is prepared by the method for preparing the mineral powder reinforced polyurethane grouting material.

[0020] The application of the mineral powder reinforced polyurethane grouting material in asphalt pavement crack repair.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention adopts polyol, isocyanate, mineral powder, curing agent and cross-linking agent to prepare mineral powder reinforced polyurethane grouting material. The performance of the polyurethane material enhanced by mineral powder not only has excellent anti-ultraviolet aging performance, but also has good durability and low-temperature stability, and can be well used in asphalt pavement crack repair.

[0023] 2. The present invention optimizes the dosage of mineral powder. When the dosage of mineral powder is 30%, the viscosity, tensile strength, elongation at break, compression strength, bonding strength and anti-ultraviolet aging comprehensive performance of the mineral powder reinforced polyurethane grouting material reach peak values, which significantly improves the mechanical properties, durability and thermal stability of the mineral powder reinforced polyurethane grouting material, and effectively reduces the maintenance cost.

[0024] 3. In the present invention, the asphalt concrete pavement crack repair performance simulation test was carried out to test the low-temperature splitting tensile strength, low-temperature bending performance test, freeze-thaw cycle splitting test and immersion Marshall stability test of the repaired asphalt mixture. The results show that:

[0025] (1) The low-temperature splitting tensile strength test shows that the splitting tensile strength of the specimens repaired with mineral powder-reinforced polyurethane grouting material can reach 75.62% compared with the original specimens. The structural stability of the repair system is good, and the effect is better than the SBS emulsified asphalt commonly used for road repair.

[0026] (2) The results of low-temperature bending tests show that the flexural tensile strength of the small beam specimens repaired with mineral powder reinforced polyurethane grouting material reaches 84.36% of the flexural tensile strength of the original specimens before damage. The repair effect is better than SBS modified asphalt and SBS emulsified asphalt commonly used for road repair.

[0027] (3) The results of freeze-thaw splitting tests show that the specimens repaired with mineral powder reinforced polyurethane grouting materials can maintain good crack resistance in cold climates, indicating that they have low-temperature stability.

[0028] (4) The results of the immersion Marshall test show that the mineral powder reinforced polyurethane grouting material has a good ability to prevent spalling when damaged by water, and the asphalt mixture repaired with the mineral powder reinforced polyurethane grouting material has good water stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the test result diagram of the elongation at break of the mineral powder reinforced polyurethane grouting material;

[0030] Figure 2 This is the test result diagram of tensile strength of polyurethane grouting material reinforced with mineral powder;

[0031] Figure 3 This is the test result diagram of the bonding strength of the polyurethane grouting material enhanced by mineral powder;

[0032] Figure 4 This is the test result diagram of the viscosity of the polyurethane grouting material reinforced with mineral powder;

[0033] Figure 5 This is the test result diagram of the compressive strength of the polyurethane grouting material reinforced with mineral powder;

[0034] Figure 6 This is a trend chart showing the effect of UV aging on tensile strength of mineral powder reinforced polyurethane grouting materials;

[0035] Figure 7 Trend chart of the effect of UV aging on elongation at break of mineral powder reinforced polyurethane grouting materials;

[0036] Figure 8 This is the Fourier infrared spectrum test result of the mineral powder reinforced polyurethane grouting material;

[0037] Fig. 9 This is a graph showing the results of thermogravimetric analysis of mineral powder reinforced polyurethane grouting materials;

[0038] Fig.10 This is a graph showing the test results of differential scanning calorimetry for mineral powder-reinforced polyurethane grouting materials;

[0039] Fig.11 Microscopic images of mineral powder-reinforced polyurethane grouting materials under fluorescence microscope and scanning electron microscope;

[0040] Fig.12 This is the result of the low temperature splitting test of the Marshall specimen after repair with the mineral powder reinforced polyurethane grouting material;

[0041] Fig.13 This is the result of the low temperature bending test of the Marshall specimen after repair with the mineral powder reinforced polyurethane grouting material;

[0042] Fig.14 This is the freeze-thaw splitting test result of the Marshall specimen after repair with mineral powder reinforced polyurethane grouting material;

[0043] Fig.15 This is the result of the submerged Marshall test of the Marshall specimen after repair with mineral powder reinforced polyurethane grouting material. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] The present invention provides a method for preparing a mineral powder reinforced polyurethane grouting material, comprising the following steps:

[0046] S1. After the polyol is subjected to vacuum dehydration treatment at a temperature of 110°C to 130°C for 1h to 2h, the temperature is lowered to about 65°C, and isocyanate is added according to a preset ratio. Then, the polyol is heated to 80°C to 85°C, and the reaction is fully carried out under nitrogen protection for 1h to 2h, and the isocyanate content is titrated. After the reaction is completed, the polyurethane prepolymer is prepared by vacuuming for 0.5h to 1h to remove the residual substances.

[0047] In this step, the content of -NCO in the polyurethane prepolymer will have different degrees of influence on the foaming effect of the polyurethane and the related properties of the solid body produced after contacting water, and the terminal -NCO polyurethane is synthesized by adding an excess of isocyanate compound. Therefore, in the process of preparing the polyurethane grouting material, it is necessary to ensure that the product contains a large amount of free -NCO after the nitrogen reaction.

[0048] During the titration process, the acetone-di-n-butylamine method in the chemical titration method is used to determine the -NCO content, and bromocresol green is used as an indicator. When the solution changes from light green to light yellow and does not return to its original color within half a minute, the titration endpoint is reached and the nitrogen protection reaction ends.

[0049] In step S1, the isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and other common isocyanates may also be selected.

[0050] In step S1, the polyol is polyether polyol (PPG), polytetramethylene ether glycol (PTMG) or polyester polyol.

[0051] In step S1, the curing agent is 4,4'-diphenyl diisocyanate (MOCA), and the addition product of toluene diisocyanate and trimethylolpropane (TDI-TMP) can also be used, and the trimer of 2,4-diisocyanato-1,6-hexamethylene diisocyanate (TDI trimer) can also be used, and other common curing agents can be selected.

[0052] In step S1, the function of the crosslinking agent is to react with isocyanate and polyol to form a three-dimensional network structure, so the selected crosslinking agent is required to have multiple functional groups. Preferably, the crosslinking agent is butanediol, glycerol or propylene glycol.

[0053] S2. Treat the polyurethane prepolymer at 80℃~90℃ for 30min~50min; that is, add mineral powder after heating for 30min~50min, stir evenly, and then treat at 80℃~90℃ for 15min~30min, that is, keep heating for 15min~30min. Then quickly stir and mix it with curing agent and cross-linking agent to obtain mineral powder reinforced polyurethane grouting material.

[0054] In this step, the added mass of the mineral powder is 10% to 40% of the mass of the urethane grouting material. Preferably, the mass fraction of the mineral powder is 10%, 20%, 30% or 40%.

[0055] Preferably, according to the mass ratio of curing agent / polyurethane prepolymer = 14.5:100, the curing agent is weighed and placed in an oven at a temperature of 110° C.-130° C. for 1.5 h to 2 h, and after the curing agent is completely liquefied, it is fully stirred and mixed with the polyurethane prepolymer.

[0056] In step S2 of the present invention, the technical indicators of the curing agent 4,4'-diphenyl diisocyanate (MOCA) are shown in Table 1.

[0057] Table 1 Technical indicators of curing agent MOCA

[0058]

[0059] In step S2 of the present invention, the crosslinking agent butanediol should be taken from the prepolymer for titration of -NCO, and then the prepolymer is evacuated for 0.5h-1h and then nitrogen is passed through and sealed for standby use. The polyurethane prepolymer is preheated, and then according to the titration result of the isocyanate content, the polyurethane prepolymer and the crosslinking agent butanediol are quickly stirred and mixed at a molar ratio of nNCO / nOH=1:1.

[0060] In the present invention, the technical indicators of the cross-linking agent butanediol are shown in Table 2.

[0061] Table 2 Technical indicators of butanediol

[0062] Relative density Chroma Refractive Index Melting point / ℃ Flash point / ℃ Boiling point / ℃ Hydroxyl value 1.017 ≤25 1.446 20.2 120 227 ≤0.2%

[0063] The present invention also provides an application of a mineral powder reinforced polyurethane grouting material in repairing cracks in an asphalt pavement. The application method includes: directly filling the cracks in the asphalt pavement with the mineral powder reinforced polyurethane grouting material.

[0064] The preparation method and performance of the mineral powder reinforced polyurethane grouting material provided by the present invention are described in detail below with reference to several groups of embodiments.

[0065] Example 1

[0066] This embodiment provides a mineral powder-reinforced polyurethane grouting material, which includes isocyanate, MOCA curing agent, butanediol cross-linking agent, 10% mineral powder and polyol.

[0067] In this embodiment, the isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyether polyol (PPG).

[0068] This embodiment provides a method for preparing a mineral powder reinforced polyurethane grouting material, comprising the following steps:

[0069] S1. After the polyol is subjected to vacuum dehydration treatment at 110°C for 1 hour, the temperature is lowered to 65°C, and isocyanate is added. Then, the mixture is heated to 80°C, and the isocyanate content is titrated after fully reacting for 1 hour under nitrogen protection. After the reaction, the mixture is vacuumed for 0.5 hour to remove the residual substances, thereby preparing a polyurethane prepolymer.

[0070] In this embodiment, the specific operation steps of the titration are as follows: first weigh a small amount of sample and place it in a conical flask, add 25mL of a mixed solution of toluene and acetone, and heat in a water bath until the sample is completely dissolved. Then, add 25mL of a 0.1mol / L di-n-butylamine-toluene solution and mix evenly, and continue to add 100mL of anhydrous ethanol after it is completely reacted; drip a few drops of bromocresol green ethanol solution as an indicator. Finally, the solution to be tested is titrated with a standard hydrochloric acid solution. When the solution color gradually changes from blue to cyan and then to light yellow, and the blue color does not recover within half a minute, the titration end point is reached. The nitrogen protection reaction is completed and vacuumized.

[0071] S2. Treat the polyurethane prepolymer at 90°C for 30 minutes, then add the mineral powder, stir evenly, and then treat it at 80°C for 30 minutes. Then quickly stir and mix it with the curing agent and the cross-linking agent to obtain the mineral powder reinforced polyurethane grouting material. The mass ratio of curing agent / polyurethane prepolymer = 14.5:100.

[0072] In this embodiment, the curing agent is first placed in an oven and treated at a temperature of 130° C. for 2 hours. After the curing agent is completely liquefied, the liquefied curing agent and the polyurethane prepolymer are fully stirred and mixed.

[0073] Example 2

[0074] This embodiment provides a mineral powder reinforced polyurethane grouting material, which includes isocyanate, MOCA curing agent, butanediol cross-linking agent, 20% mineral powder and polyol.

[0075] In this embodiment, the isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyether polyol (PPG).

[0076] Example 3

[0077] This embodiment provides a mineral powder reinforced polyurethane grouting material, which includes isocyanate, MOCA curing agent, butanediol cross-linking agent, 30% mineral powder and polyol.

[0078] In this embodiment, the isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyether polyol (PPG).

[0079] Example 4

[0080] This embodiment provides a mineral powder reinforced polyurethane grouting material, which includes isocyanate, MOCA curing agent, butanediol cross-linking agent, 40% mineral powder and polyol.

[0081] In this embodiment, the isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyether polyol (PPG).

[0082] Embodiment 5 to Embodiment 8

[0083] The difference from Examples 1 to 4 is that the polyol used is polytetramethylene ether glycol (PTMEG).

[0084] Embodiment 9 to Embodiment 12

[0085] The difference from Examples 1 to 4 is that the polyol used is polyester polyol.

[0086] From the above, it can be seen that in Examples 1 to 4, the polyol used is polyether polyol, and the mineral powder-reinforced polyurethane grouting materials are obtained at different mass mineral powder dosages (10%, 20%, 30% and 40%); in Examples 5 to 8, the polyol used is polytetramethylene ether glycol, and the mineral powder-reinforced polyurethane grouting materials are obtained at different mass mineral powder dosages (10%, 20%, 30% and 40%); in Examples 9 to 12, the polyol used is polyester polyol, and the mineral powder-reinforced polyurethane grouting materials are obtained at different mineral powder dosages (10%, 20%, 30% and 40%).

[0087] Comparative Example 1

[0088] In this comparative example, no mineral powder was added, and the rest was the same as in Example 1.

[0089] This comparative example provides a mineral powder reinforced polyurethane grouting material, comprising isocyanate, polyol, MOCA curing agent and butanediol crosslinking agent. The isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyether polyol (PPG).

[0090] Comparative Example 2

[0091] In this comparative example, no mineral powder was added, and the rest was the same as in Example 5.

[0092] This comparative example provides a mineral powder reinforced polyurethane grouting material, comprising isocyanate, polyol, MOCA curing agent and butanediol crosslinking agent. The isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polytetramethylene ether glycol (PTMEG).

[0093] Comparative Example 3

[0094] In this comparative example, no mineral powder was added, and the rest was the same as in Example 9.

[0095] This comparative example provides a mineral powder reinforced polyurethane grouting material, comprising isocyanate, polyol, MOCA curing agent and butanediol crosslinking agent. The isocyanate is diphenylmethane-4,4'-diisocyanate (MDI), and the polyol is polyester polyol.

[0096] Furthermore, the performance of the mineral powder reinforced polyurethane grouting materials prepared in the above examples and comparative examples was verified.

[0097] Test 1

[0098] In order to explore the optimal mineral powder dosage and raw materials of mineral powder reinforced polyurethane grouting materials, and have a clearer understanding of its physical indicators, mechanical properties and aging resistance.

[0099] This experiment used fifteen kinds of mineral powder reinforced polyurethane grouting materials prepared by Examples 1 to 12 and Comparative Examples 1 to 3, among which the mineral powder reinforced polyurethane grouting materials of Examples 1 to 4 and Comparative Example 1 were recorded as mineral powder reinforced polyurethane grouting material I, the mineral powder reinforced polyurethane grouting materials of Examples 5 to 8 and Comparative Example 2 were recorded as mineral powder reinforced polyurethane grouting material II, and the mineral powder reinforced polyurethane grouting materials of Examples 9 to 12 and Comparative Example 3 were recorded as mineral powder reinforced polyurethane grouting material III.

[0100] The viscosity, tensile strength, elongation at break, compression strength, bonding strength and UV aging resistance of the adhesive were studied. The results are shown in the attached Figure 1 to Figure 7 shown.

[0101] The viscosity of polyurethane is measured according to the method for measuring the viscosity of adhesives in GB / T-2794-2022; the tensile strength and elongation at break are tested according to GB / T528-2009; the compressive strength of polyurethane grouting materials is tested according to the compression test method specified in GB / T2567-2021.

[0102] Depend on Figure 1 to Figure 5It can be seen that when the mineral powder content gradually increases, the elongation at break of the mineral powder-reinforced polyurethane grouting material decreases, and the change trend of the tensile strength and bonding performance is first increased and then decreased, reaching a peak value when the mineral powder content is 30%. The results of the study on mortar viscosity and compression performance show that the mortar viscosity and compression strength of the mineral powder-reinforced polyurethane grouting material increase, but the growth rate gradually slows down. When the mineral powder content exceeds 30%, the slowing trend is particularly obvious. From the above experimental results, it can be concluded that the mineral powder-reinforced polyurethane grouting material prepared by PPG and MDI has the best comprehensive performance, and its optimal mineral powder content is 30%.

[0103] Depend on Figure 6 and Figure 7 It can be seen that the tensile properties of the polyurethane grouting material enhanced by mineral powder have been greatly improved after 3 days of UV aging, with an increase of 36.91%, and the tensile strength has reached 19.09MPa. After UV aging, the polyurethane grouting material enhanced by mineral powder can still maintain good performance. This proves that the addition of mineral powder can not only reduce the cost of the polyurethane grouting material enhanced by mineral powder, but also improve its mechanical properties and anti-UV aging performance.

[0104] Test 2

[0105] In order to study the microscopic mechanism and characteristics of the mineral powder reinforced polyurethane grouting material, this experiment selected the mineral powder reinforced polyurethane grouting materials of Examples 1 to 4 and Comparative Example 1 for experimental observation.

[0106] This test specifically verifies the performance through Fourier transform infrared spectroscopy (FTIR) test, thermogravimetric analysis (TG) test, and differential scanning calorimetry (DSC) test.

[0107] See also Figure 8 The Fourier transform infrared spectrum images show that the addition of mineral powder has no effect on the overall structure of the mineral powder reinforced polyurethane grouting material.

[0108] See also Fig. 9 The results of thermogravimetric analysis show that the introduction of mineral powder improves the thermal stability of mineral powder-reinforced polyurethane grouting materials.

[0109] See also Fig.10 The DSC differential results prove that the mineral powder reinforced polyurethane grouting material still has good thermal stability after UV aging.

[0110] In addition, the materials of Example 3 (mineral powder content 30%), Example 4 (mineral powder content 40%) and Comparative Example 1 (no mineral powder added) were tested by fluorescence microscopy and electron microscopy scanning. The results are as follows: Fig.11 As shown, the green on the left is the fluorescence image, and the gray on the right is the scanning electron microscopy result.

[0111] from Fig.11 It can be seen from the fluorescence microscope images and scanning electron microscope images that when the mineral powder dosage is 30%, the mineral powder is evenly distributed in the mineral powder enhanced polyurethane grouting material and the dispersion effect is good. When it is added as a component to the mineral powder enhanced polyurethane grouting material, the mineral powder enhanced polyurethane grouting material is effectively enhanced.

[0112] Test 3

[0113] In order to study the crack repairing performance of asphalt concrete pavement with mineral powder reinforced polyurethane grouting material, mineral powder reinforced polyurethane grouting material, SBS modified asphalt and SBS emulsified asphalt were used as crack repairing materials, and the repaired asphalt mixtures were subjected to low-temperature splitting test, low-temperature bending test, freeze-thaw splitting test and immersion Marshall test.

[0114] In this test, the mineral powder-reinforced polyurethane grouting material was prepared in Example 3; at the same time, SBS modified asphalt and SBS emulsified asphalt commonly used for road repair on the market were used for comparison.

[0115] In the test, a standard Marshall specimen of asphalt mixture was prepared to simulate road cracks. The original specimen was cut into two halves, and then a 5mm crack width was simulated. The above three materials were used to repair the cracks. The mineral powder in the Marshall specimen was limestone mineral powder produced by a building materials factory. The technical indicators of the mineral powder are shown in Table 3.

[0116] Table 3 Technical indicators of mineral powder

[0117] Inspection items Test value Require Test methods Appearance No lumps No lumps Observational method Particle size ≤0.6mm / % 100 - Sieving method Particle size ≤0.15mm / % 97.2 - Sieving method Particle size ≤0.075mm / % 87.3 - Sieving method Hydrophilicity 0.7 <1 T0353-2000 Plasticity Index 3.8 <4 T0354-2000 <![CDATA[Apparent relative density (g / cm -3 )]]> 2.74 ≥2.50 T0352-2000 Water content / % 0.5 ≤1 T0103 Drying method

[0118] In this test, the asphalt used was Donghai A-70 asphalt, and its technical indicators are shown in Table 4.

[0119] Table 4 Technical indicators of Donghai A-70 asphalt

[0120] Inspection items Quality indicators Test results Test methods Needle penetration (25℃) / 0.1mm 60-80 67 T0604 Penetration Index PI -1.5-1.0 -0.51 T0604 Softening point / ℃ ≥46 48.7 T0606 60℃ dynamic viscosity, Pa.s ≥180 231 T0620 Elongation (15℃) / cm ≥15 24 T0605 Elongation (25℃) / cm ≥100 >100 T0605 Flash point / ℃ ≥260 271 T0611 Solubility / % ≥99.5 99.81 T0607 <![CDATA[Density / (g·cm -3 )]]> ---- 1.01 T0603

[0121] In this test, the specimens were graded AC-13, and the screening test results are shown in Table 5.

[0122] Table 5 Screening test results used in the test

[0123]

[0124]

[0125] In this test, the optimal asphalt dosage of the specimen is 4.7%.

[0126] Depend on Fig.12 and Fig.13It can be seen that the low-temperature splitting test proves that the splitting tensile strength of the specimens repaired with the mineral powder reinforced polyurethane grouting material can reach 75.62% compared with the original specimens, the structural stability of the repair system is good, and the repair effect is better than SBS emulsified asphalt; the low-temperature bending test proves that the bending tensile strength of the small beam specimens repaired with the mineral powder reinforced polyurethane grouting material reaches 84.36% of the bending tensile strength of the original specimens before damage, and the repair effect is better than SBS modified asphalt and SBS emulsified asphalt. The mineral powder reinforced polyurethane grouting material has good mechanical compatibility with the damaged small beam specimens, the repaired small beam specimens have a large critical stress for cracking, good recovery effect, good structural stability, can resist large bending tensile stress, and the repaired asphalt mixture has good low-temperature stability.

[0127] Depend on Fig.14 and Fig.15 It can be seen that the freeze-thaw splitting test proves that the freeze-thaw splitting tensile strength ratio TSR of the specimen with a crack width of 5mm after being repaired by the mineral powder reinforced polyurethane grouting material is 85.92%, which is better than the mainstream normal temperature crack repair material SBS emulsified asphalt. The specimens repaired by the mineral powder reinforced polyurethane grouting material can maintain good crack resistance in cold climates. The residual stability of the Marshall specimen with a crack width of 5mm after being repaired by the mineral powder reinforced polyurethane grouting material is 87.37%, which is higher than SBS modified asphalt and SBS emulsified asphalt. The immersion Marshall test shows that the mineral powder reinforced polyurethane grouting material has a good ability to prevent peeling when damaged by water, and the asphalt mixture has good water stability after repair.

[0128] The above test verifies that the mineral powder reinforced polyurethane grouting material provided by the present invention, the mineral powder reinforced polyurethane grouting material prepared from polyol PPG, polyurethane MDI and mineral powder, has the best comprehensive performance, and the optimal mineral powder dosage is 30%, which can effectively improve the economy, mechanical properties, durability and thermal stability of polyurethane materials. And compared with traditional polyurethane materials, the mineral powder reinforced polyurethane grouting material shows more superior performance in anti-ultraviolet aging performance, and shows excellent low temperature stability and water stability in crack repair applications.

[0129] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a mineral powder-reinforced polyurethane grouting material, It is characterized in that The following steps are involved: S1. Preparation of polyurethane prepolymer In a nitrogen atmosphere, a polyurethane prepolymer is prepared by using polyol and isocyanate; S2. Preparation of mineral powder reinforced polyurethane grouting material The polyurethane prepolymer of step S1 is pretreated, and then mineral powder is added and mixed evenly; after being treated again, it is mixed with a curing agent and a cross-linking agent to obtain an urethane grouting material; the mass of the added mineral powder is 10% to 40% of the mass of the urethane grouting material; the mass ratio of the curing agent to the polyurethane prepolymer is 14.5:100; and the molar ratio of the cross-linking agent to the polyurethane prepolymer is 1:

1.

2. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 1, It is characterized in that In the step S2, the curing agent is an addition product of toluene diisocyanate and trimethylolpropane, 4,4'-diisocyanate diphenyl ester, or 2,4-diisocyanato-1,6-hexamethylene diisocyanate trimer; and the cross-linking agent is butanediol, glycerol or propylene glycol.

3. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 1, It is characterized in that The pretreatment is carried out at a temperature of 80°C to 90°C for 30 minutes to 50 minutes; the secondary treatment is carried out at a temperature of 80°C to 90°C for 15 minutes to 30 minutes.

4. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 1, It is characterized in that In step S1, the preparation process of the polyurethane prepolymer is: The polyol is vacuum dehydrated and cooled, then mixed with isocyanate, heated, fully reacted under a nitrogen atmosphere, and then vacuumed to obtain a polyurethane prepolymer.

5. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 4, It is characterized in that The polyol is polyether polyol, polytetramethylene ether glycol or polyester polyol.

6. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 4, It is characterized in that The vacuum dehydration and cooling process is to carry out vacuum dehydration treatment at a temperature of 110° C. to 130° C. for 1 h to 2 h, and then reduce the temperature to 65° C.

7. The method for preparing the mineral powder reinforced polyurethane grouting material according to claim 4, It is characterized in that The heating temperature is 80°C to 85°C, the reaction is fully carried out for 1h to 2h, and the vacuum is applied for 0.5h to 1h.

8. The mineral powder reinforced polyurethane grouting material prepared by the preparation method of the mineral powder reinforced polyurethane grouting material according to claim 1.

9. Use of the mineral powder reinforced polyurethane grouting material as claimed in claim 8 in repairing cracks in asphalt pavement.

Citation Information

Cited By

  • Polyurethane grouting material and preparation method thereof

    CN122483294A