Liquid N-phenyl naphthylamine derivative high-temperature antioxidant and preparation method thereof
The liquid alkylated N-phenylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylnaphthylna The problems of α-naphthylamine in high temperatures improve oxidation resistance and thermal stability, simplify operation and achieve faster reaction rates.
Patent Information
- Application Number
- CN202411058568.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
The existing N-phenyl-α-naphthylamine is prone to sludge and precipitation under high temperature conditions, and there are problems of dust pollution and complex industrial production during the use of solid additives.
By introducing a small amount of N-phenyl-β-naphthaleneamine and controlling its added amount, a liquid N-phenylnaphthaleneamine derivative with a special structural distribution is formed, and a phosphoric acid/nitric acid modified Elolite catalyst and poly-resistance inhibitor are used. The agent is alkylated and prepared a liquid alkylated N-phenylnaphthylnaphthylamine derivative high-temperature antioxidant, avoiding poor solubility of solid additives and oil sludge problems.
Improves antioxidant properties and thermal stability, simplifies operation, avoids dust contamination, and achieves faster reaction rates under milder conditions.
Smart Images

Figure CN118956464A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of antioxidants, in particular to a liquid N-phenylnaphthylamine derivative high-temperature antioxidant and a preparation method of the liquid N-phenylnaphthylamine derivative high-temperature antioxidant. Background Art
[0002] N-phenyl-α-naphthylamine is widely used in lubricant additives and rubber fields because it has good antioxidant properties at high working temperatures. However, N-phenyl-α-naphthylamine is prone to produce more sludge and precipitation during use as a lubricant additive, making it difficult to meet the requirements of some working conditions.
[0003] The prior art discloses that a solid alkylated N-phenyl-α-naphthylamine antioxidant is prepared by alkylating N-phenyl-α-naphthylamine with diisobutylene, and the antioxidant has not only good antioxidant properties under high temperature conditions, but also has a low tendency to form sludge. However, compared with liquid additives, solid additives have many inconveniences during use, such as the need for additional processing when feeding, and solid feeding is prone to dust pollution.
[0004] Based on the advantages of liquid antioxidants, the prior art also discloses a method for preparing liquid antioxidants, but the preparation method is relatively complicated and is not conducive to industrial production.
[0005] In addition, there is a prior art disclosure of a method for preparing alkylated N-phenyl-α-naphthylamine, in which anhydrous aluminum chloride is used as a catalyst, and isopentene and N-phenyl-α-naphthylamine are used to prepare alkylated N-phenyl-α-naphthylamine. However, this method produces a large amount of acidic waste water, and it is difficult to fully extract the target product from the reaction solution. The actual yield is only 23% of the theoretical yield. Summary of the invention
[0006] In view of the above problems, the present invention provides a liquid N-phenylnaphthylamine derivative high-temperature antioxidant and a preparation method thereof. By introducing a small amount of N-phenyl-β-naphthylamine and regulating its addition amount, the proportions of different components in the product are adjusted to form an N-phenylnaphthylamine derivative composition that is liquid at room temperature and has a special structural distribution, thereby effectively improving the antioxidant performance and thermal stability of the mixture, effectively overcoming the shortcomings of poor solubility of solid additives and easy generation of sludge and precipitation during use, and compared with solid additives, no additional processing and additional heating are required, and dust pollution will not be caused. Moreover, the catalyst can provide more active sites for the reaction, which is beneficial to the transfer of electrons, so that the reaction can be carried out at a faster reaction rate under milder conditions.
[0007] To achieve the above object, the present invention provides a liquid N-phenylnaphthylamine derivative high temperature antioxidant, which comprises, by mass percentage:
[0008] At least 98 wt% of a mixture of alkylated and arylated N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines, and less than 2 wt% of a mixture of unsubstituted N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines.
[0009] The present invention also provides a method for preparing a liquid N-phenylnaphthylamine derivative high-temperature antioxidant, which is used to prepare the liquid N-phenylnaphthylamine derivative high-temperature antioxidant disclosed in the above technical solution, comprising:
[0010] Adding N-phenyl-α-naphthylamine, a phosphoric acid / nitric acid modified halloysite catalyst and a polymerization inhibitor into a closed reactor, and removing moisture from the reactor;
[0011] Adding olefin dropwise into the reaction kettle to carry out alkylation reaction;
[0012] After adding N-phenyl-β-naphthylamine to the reaction kettle, olefin is added dropwise again;
[0013] The acidic solid catalyst in the reactor is removed by filtration, and unreacted olefins are removed by reduced pressure distillation to obtain a liquid alkylated N-phenylnaphthylamine derivative high-temperature antioxidant.
[0014] In the above technical solution, preferably, the preparation process of the phosphoric acid / nitric acid modified halloysite catalyst comprises:
[0015] Halloysite is added into a mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 hours, filtered, and the filter cake is dried at 100° C., ground and passed through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst;
[0016] The mass fraction ratio of phosphoric acid to nitric acid is 1:1, and the total concentration of phosphoric acid and nitric acid is 10-30wt%;
[0017] Wherein, the addition amount of the phosphoric acid / nitric acid modified halloysite catalyst is 5% to 30% of the total mass of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine.
[0018] In the above technical solution, preferably, the polymerization inhibitor includes hydroquinone, tert-butylcatechol, 2,6-dinitro-p-cresol and 2,5-di-tert-amylhydroquinone, and the addition amount of the polymerization inhibitor is 30 to 150 ppm.
[0019] In the above technical solution, preferably, the olefin is selected from tripropylene, tetrapropylene or styrene, and the olefin is added all at once or in batches for multiple times, and the styrene accounts for 0 to 10% of the total molar amount of the olefin;
[0020] The molar ratio of the total amount of the olefin added to the total amount of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine is 2.5:1 to 6:1.
[0021] In the above technical solution, preferably, the N-phenyl-β-naphthylamine accounts for 0 to 20% of the total molar amount of the N-phenyl-α-naphthylamine and the N-phenyl-β-naphthylamine.
[0022] In the above technical solution, preferably, the filter cake is collected and processed and then recycled as a catalyst, and the olefin removed by vacuum distillation is used as a raw material to participate in the reaction cycle.
[0023] In the above technical solution, preferably, the specific operation of removing the water in the reactor includes:
[0024] Using nitrogen to replace the air in the closed reactor;
[0025] The reactor was heated until the temperature reached 70° C., and the stirring and vacuum systems of the reactor were turned on;
[0026] When the temperature rises to 100° C., the temperature is kept for half an hour to remove the moisture in the reactor;
[0027] The vacuum system was stopped, and the reactor was replaced with nitrogen to a normal pressure state.
[0028] In the above technical solution, preferably, during the alkylation reaction, the olefin is added dropwise within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.
[0029] In the above technical solution, preferably, after adding N-phenyl-β-naphthylamine to the reactor, the olefin added again is added dropwise within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.
[0030] Compared with the prior art, the present invention has the following beneficial effects: by introducing a small amount of N-phenyl-β-naphthylamine and regulating the amount of N-phenyl-β-naphthylamine added, the proportions of different components in the product are adjusted to form an N-phenylnaphthylamine derivative composition which is liquid at room temperature and has a special structural distribution, the antioxidant performance and thermal stability of the mixture are effectively improved, and the shortcomings of poor solubility of solid additives and easy generation of sludge and precipitation during use are effectively overcome. Compared with solid additives, no additional processing and additional heating are required, and dust pollution will not be caused. Moreover, the catalyst can provide more active sites for the reaction, which is beneficial to the transfer of electrons, so that the reaction can be carried out at a faster reaction rate under milder conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1A transmission electron microscope image of halloysite disclosed in one embodiment of the present invention;
[0032] Figure 2 This is a schematic diagram of thermogravimetric analysis of the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative composition synthesized in Example 3 of the present invention;
[0033] Figure 3 The figure is a schematic diagram of thermogravimetric analysis of a commercially available alkylated N-phenyl-α-naphthylamine of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0036] According to the present invention, a liquid N-phenylnaphthylamine derivative high-temperature antioxidant is provided, which comprises, by mass percentage:
[0037] At least 98 wt% of a mixture of alkylated and arylated N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines, and less than 2 wt% of a mixture of unsubstituted N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines.
[0038] In this embodiment, a small amount of N-phenyl-β-naphthylamine is introduced and its addition amount is controlled and limited to adjust the ratio of alkylated and arylalkylated N-phenyl-α-naphthylamine to alkylated and arylalkylated N-phenyl-β-naphthylamine in the product to form a liquid N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative composition having a special structural distribution at room temperature. The reason is that the synthetic product has many asymmetric special structures, and this special structural distribution can prevent crystallization and maximize the antioxidant performance of the mixture.
[0039] In addition, the introduction of N-phenyl-β-naphthylamine can effectively improve the thermal stability of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions.
[0040] Compared with solid additives, the liquid N-phenylnaphthylamine derivative composition does not require additional processing when preparing oil products, does not cause dust pollution, does not require additional energy consumption for heating, simplifies operation and saves energy.
[0041] The present invention also provides a method for preparing a liquid N-phenylnaphthylamine derivative high-temperature antioxidant, which is used to prepare the liquid N-phenylnaphthylamine derivative high-temperature antioxidant disclosed in the above embodiment, comprising:
[0042] Add N-phenyl-α-naphthylamine, phosphoric acid / nitric acid modified halloysite catalyst and polymerization inhibitor into a closed reactor, and remove moisture from the reactor;
[0043] Add olefin dropwise into the reaction kettle to carry out alkylation reaction;
[0044] After adding N-phenyl-β-naphthylamine to the reaction kettle, olefin was added dropwise again;
[0045] The acidic solid catalyst in the reaction kettle is removed by filtration, and the unreacted olefin is removed by reduced pressure distillation to obtain a liquid alkylated N-phenylnaphthylamine derivative high-temperature antioxidant.
[0046] In this embodiment, a small amount of N-phenyl-β-naphthylamine is introduced and its addition amount is controlled to adjust the proportion of different components in the product to form an N-phenylnaphthylamine derivative composition that is liquid at room temperature and has a special structural distribution, thereby effectively improving the antioxidant properties and thermal stability of the mixture, effectively overcoming the shortcomings of poor solubility of solid additives and easy generation of sludge and precipitation during use. Compared with solid additives, no additional processing and additional heating are required, and dust pollution will not be caused. The catalyst can provide more active sites for the reaction, which is beneficial to the transfer of electrons, so that the reaction can be carried out at a faster reaction rate under milder conditions.
[0047] In the implementation process, the alkylated and aralkylated N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions prepared by the present invention can be applied to polymer additives and lubricant additives. The mixture can exhibit excellent high-temperature antioxidant performance in turbine oil as a lubricant antioxidant, effectively improving the shortcomings of short service life and high precipitation of lubricant oil in the presence of metals.
[0048] In the above embodiment, preferably, the specific operation of removing water from the reaction kettle includes:
[0049] The air in the closed reactor is replaced by nitrogen;
[0050] Heat the reactor until the temperature rises to 70°C, and start the stirring and vacuum systems of the reactor;
[0051] When the temperature rises to 100°C, keep it for half an hour to remove the moisture in the reactor;
[0052] The vacuum system was stopped and the reactor was replaced with nitrogen to normal pressure.
[0053] In the above embodiment, preferably, during the alkylation reaction, the olefin is added dropwise within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.
[0054] In the above embodiment, preferably, after adding N-phenyl-β-naphthylamine to the reactor, the olefin is added again within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.
[0055] In the above embodiment, preferably, the preparation process of the phosphoric acid / nitric acid modified halloysite catalyst comprises:
[0056] Halloysite is added into a mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 hours, filtered, and the filter cake is dried at 100° C., ground and passed through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst;
[0057] Wherein, the mass fraction ratio of phosphoric acid to nitric acid is 1:1, and the total concentration of phosphoric acid and nitric acid is 10-30wt%, preferably 20wt%;
[0058] The addition amount of the phosphoric acid / nitric acid modified halloysite catalyst is 5% to 30% of the total mass of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine.
[0059] Specifically, compared with the commonly used activated clay catalyst, halloysite is a natural aluminosilicate mineral material, which is environmentally friendly, pollution-free, cheap and easy to obtain. Compared with activated clay, the halloysite nanotubes with a hollow tubular structure have a larger specific surface area and can provide more active sites for the reaction. In addition, the inside and outside of the halloysite nanotubes have opposite electronegativity, which is conducive to electron transfer. Therefore, the nitric acid / phosphoric acid modified halloysite catalyst can complete the alkylation reaction faster under milder conditions. Not only that, the catalyst can be reused by simple sedimentation filtration, the post-processing is not complicated, and no three wastes are generated.
[0060] According to Figure 1 The transmission electron microscope image of halloysite shown in the figure shows that halloysite has a hollow tubular structure, in which the tube length is 1 to 2 μm and the tube diameter is 100 to 150 nm. The unique hollow tubular structure of halloysite gives it a large specific surface area, which can provide more reaction sites for the alkylation reaction, facilitate the transfer of electrons, and enable the reaction to proceed quickly under mild conditions.
[0061] In the above embodiment, preferably, the polymerization inhibitor includes hydroquinone, tert-butylcatechol, 2,6-dinitro-p-cresol and 2,5-di-tert-amylhydroquinone, and the amount of the polymerization inhibitor added is based on the amount of olefin added, preferably 30 to 150 ppm.
[0062] In the above embodiment, preferably, the olefin is selected from tripropylene, tetrapropylene or styrene, and the olefin is added all at once or in batches, and the styrene accounts for 0 to 10% of the total molar amount of the olefin;
[0063] The molar ratio of the total amount of olefin added to the total amount of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine is 2.5:1 to 6:1.
[0064] In the above embodiment, preferably, N-phenyl-β-naphthylamine accounts for 0 to 20% of the total molar amount of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine.
[0065] In the above embodiment, preferably, the filter cake is collected and processed and then recycled as a catalyst, and the olefins removed by vacuum distillation are recycled as raw materials to participate in the reaction.
[0066] The N-phenylnaphthylamine derivative composition prepared according to the preparation method can remain in a liquid state for a long time at a relatively low ambient temperature, wherein the low temperature refers to 15°C, 5°C, 0°C or even lower.
[0067] The N-phenylnaphthylamine derivative composition has good oil solubility, that is, after being added into finished oil at a certain dosage, it can remain stable for a long time and the oil will not become turbid, and the long time refers to more than 1 year.
[0068] In the implementation process, the liquid N-phenylnaphthylamine derivative high temperature antioxidant and the preparation method of the present invention are described in more detail through the following examples.
[0069] Example 1
[0070] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 15 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0071] Add 40g of N-phenyl-α-naphthylamine, 15g of nitric acid / phosphoric acid modified halloysite catalyst, and 60ppm of inhibitor hydroquinone to a stainless steel reactor, introduce nitrogen into the closed reactor, fully replace the air in the reactor, and start heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa to 0.095MPa. When the temperature reaches about 70°C, start stirring, and the stirring rate is 300 rpm. When the temperature rises to 100°C, keep it warm for half an hour to remove the moisture in the reaction system, then stop the vacuum system, replace the reactor with nitrogen to normal pressure, and drop 95.95g of tetrapropylene into the reactor. The feeding time is controlled within 30min. After the feeding is completed, continue to heat to 150°C and react at a constant temperature for 6h; then add 10g of N-phenyl-β-naphthylamine, continue to react for 6h, and then stop the reaction. When the temperature of the reaction system drops to room temperature, release the product in the reactor for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to vacuum distillation to recover excess olefins, and the recovered olefins can be further recycled as raw materials. The vacuum degree of the vacuum distillation is about 0.095 MPa, the temperature is 190°C, and the light brown liquid obtained by the vacuum distillation is a composition derived from N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine. According to chromatographic analysis, the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine in the product is 1.13%.
[0072] Example 2
[0073] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 20 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0074] Add 45g of N-phenyl-α-naphthylamine, 15g of nitric acid / phosphoric acid modified halloysite catalyst, and 65ppm of inhibitor hydroquinone to a stainless steel reactor, introduce nitrogen into the closed reactor, fully replace the air in the reactor, and start heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa-0.095MPa. When the temperature reaches about 70°C, start stirring, and the stirring rate is 350 rpm. When the temperature rises to 100°C, keep warm for half an hour to remove the moisture in the reaction system, then stop the vacuum system, and replace the reactor with nitrogen to normal pressure; add 134.33g of tetrapropylene to the reactor, and the feeding time is controlled within 30min. After the feeding is completed, continue to heat to 150°C and react at a constant temperature for 12h; then add 57.57g of tetrapropylene and 5g of N-phenyl-β-naphthylamine to the reactor, continue to react for 6h, and then stop the reaction, and the feeding time is controlled within 30min. When the temperature of the reaction system drops to room temperature, the product in the reactor is released for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to reduced pressure distillation to recover excess olefins, and the recovered olefins can be further recycled as raw materials. The vacuum degree of reduced pressure distillation is about 0.095MPa, and the temperature is 190°C. The light brown liquid obtained by reduced pressure distillation is a derivative composition of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine. According to chromatographic analysis, the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine in the product is 0.93%.
[0075] Example 3
[0076] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 20 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0077] Add 45g of N-phenyl-α-naphthylamine, 15g of nitric acid / phosphoric acid modified halloysite catalyst, and 75ppm of inhibitor 2,6-dinitro-p-cresol into a stainless steel reactor, introduce nitrogen into the closed reactor, fully replace the air in the reactor, and start heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa-0.095MPa. When the temperature reaches about 70°C, start stirring at a stirring rate of 300 rpm. When the temperature rises to 100°C, keep warm for half an hour to remove the moisture in the reaction system, then stop the vacuum system, and replace the reactor with nitrogen to normal pressure; add 191.90g of tetrapropylene to the reactor, and control the feeding time within 30min. After the feeding is completed, continue to heat to 160°C and react at a constant temperature for 12h; then add 11.87g of styrene and 5g of N-phenyl-β-naphthylamine to the reactor, continue to react for 6h, then stop the reaction, and control the feeding time within 30min. When the temperature of the reaction system drops to room temperature, the product in the reactor is discharged for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to vacuum distillation to recover excess olefins, and the recovered olefins can be further recycled as raw materials. The vacuum degree of vacuum distillation is about 0.095MPa, and the temperature is 190°C. The light brown liquid obtained by vacuum distillation is a derivative composition of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine, and the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine is 0.57%.
[0078] Example 4
[0079] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 10 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0080] Add 40g of N-phenyl-α-naphthylamine, 10g of nitric acid / phosphoric acid modified halloysite catalyst, and 60ppm of inhibitor 2,5-di-tert-amylhydroquinone to a stainless steel reactor, and introduce nitrogen into the closed reactor to fully replace the air in the reactor before starting heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa to 0.095MPa. When the temperature reaches about 70°C, start stirring at a stirring rate of 300 rpm. When the temperature rises to 100°C, keep warm for half an hour to remove moisture from the reaction system, then stop the vacuum system, and replace the reactor with nitrogen to normal pressure; drop 152.5g of nonene into the reactor, and control the feeding time within 30min. After the feeding is completed, continue to heat to 180°C and react at a constant temperature for 6h; then add 10g of N-phenyl-β-naphthylamine, continue to react for 6h, and then stop the reaction. When the temperature of the reaction system drops to room temperature, the product in the reactor is released for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to reduced pressure distillation to recover excess olefins, and the recovered olefins can be further recycled as raw materials. The vacuum degree of reduced pressure distillation is about 0.095MPa, and the temperature is 190°C. The light brown liquid obtained by reduced pressure distillation is a derivative composition of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine. According to chromatographic analysis, the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine in the product is 1.02%.
[0081] Example 5
[0082] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 10 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0083] Add 40g of N-phenyl-α-naphthylamine, 14g of nitric acid / phosphoric acid modified halloysite catalyst, 90ppm inhibitor tert-butyl catechol into a stainless steel reactor, introduce nitrogen into the reactor, fully replace the air in the reactor, and start heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa to 0.095MPa. When the temperature reaches about 70°C, start stirring, the stirring rate is 300 rpm, and remove the moisture in the reaction system under vacuum conditions. Gradually heat to 100°C and keep warm for half an hour, then stop the vacuum system and replace it with nitrogen to normal pressure; add 172.7g of tetrapropylene to the reactor, control the feeding time to 30min, continue to increase the temperature to 160°C and react at a constant temperature for 12 hours, then add 11.87g of styrene and 10g of N-phenyl-β-naphthylamine to the reactor, continue to react for 12 hours, and then stop the reaction. When the temperature of the reaction system drops to room temperature, the product in the reactor is discharged for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to vacuum distillation to recover the excess tetrapropylene, and the recovered olefin can be further recycled as a raw material. The vacuum degree of vacuum distillation is about 0.095MPa, and the temperature is 190°C. The light brown liquid obtained by vacuum distillation is a derivative composition of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine. According to chromatographic analysis, the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine in the product is 1.32%.
[0084] Example 6
[0085] 100 g of halloysite was dispersed in a three-necked flask containing 250 ml of a 25 wt% mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 h, and then filtered. The filter cake was dried at 100° C. for 12 h, ground, and sieved through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst.
[0086] Add 45g of N-phenyl-α-naphthylamine, 10g of nitric acid / phosphoric acid modified halloysite catalyst, 50ppm inhibitor tert-butyl catechol into a stainless steel reactor, introduce nitrogen into the reactor, fully replace the air in the reactor, and start heating. At the same time, turn on the vacuum system, and control the vacuum degree in the reactor at 0.08MPa-0.095MPa. When the temperature reaches about 70°C, start stirring, the stirring rate is 300 rpm, and remove the moisture in the reaction system under vacuum conditions. Gradually heat to 100°C and keep warm for half an hour, then stop the vacuum system and replace it with nitrogen to normal pressure; add 225.2g of tetrapropylene to the reactor, control the feeding time within 30min, continue to heat to 180°C and react at a constant temperature for 6h, then add 5g of N-phenyl-β-naphthylamine, continue to react for 6h and stop the reaction. When the temperature of the reaction system drops to room temperature, release the product in the reactor for filtration, and the filter cake can be reused as a catalyst. The filtered mother liquor is subjected to vacuum distillation to recover excess olefins, and the recovered olefins can be further recycled as raw materials. The vacuum degree of the vacuum distillation is 0.095 MPa and the temperature is 190° C. The light brown liquid obtained by the vacuum distillation is a composition derived from N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine. According to chromatographic analysis, the total content of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine in the product is 1.77%.
[0087] Commercially available alkylated N-phenyl-α-naphthylamine and the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in Examples 1 to 3 above were prepared into ordinary turbine oil 1, ordinary turbine oil 2, improved turbine oil 1, improved turbine oil 2, and improved turbine oil 3 according to the same formula. The oxidation stability test was carried out in accordance with the "Determination of oxidation stability of lubricating oil by rotating oxygen bomb method RPVOT BVOT" SH / T 0193. This test is to place the sample, water and copper catalyst coil into an oxygen bomb, and evaluate the oxidation stability of the sample by detecting the time required for the sample to reach a specified pressure drop due to oxidation. This test focuses on the antioxidant performance of the oil under metal catalysis. The longer the oxidation life, the better the antioxidant effect. The test results are shown in Table 1 below:
[0088] Table 1 Oxidation stability test results
[0089] Turbine oil batch number Oxidation life / min Ordinary turbine oil 1 1025 Ordinary turbine oil 2 1057 Improved turbine oil 1 1145 Improved turbine oil 2 1177 Improved turbine oil 3 1193
[0090] It can be seen from the above test results that the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions prepared by the present invention exhibit a longer oxidation life when formulated into lubricating oils. Compared with the alkylated N-phenyl-α-naphthylamine currently sold on the market, the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions prepared by the present invention have better antioxidant properties.
[0091] The oil solubility test was conducted on the above five batches of oil products, that is, the above oil products were placed at room temperature to observe their stability. The results are shown in Table 2 below.
[0092] Table 2 Oil solubility test results
[0093] Turbine oil batch number Initial state Three months One year Ordinary turbine oil 1 Clear and transparent Clear and transparent Turbidity appears Ordinary turbine oil 2 Clear and transparent Clear and transparent Turbidity appears Improved turbine oil 1 Clear and transparent Clear and transparent Clear and transparent Improved turbine oil 2 Clear and transparent Clear and transparent Clear and transparent Improved turbine oil 3 Clear and transparent Clear and transparent Clear and transparent
[0094] It can be seen from the above test results that the N-phenyl-α-naphthylamine mixture prepared by the present invention has good oil solubility. When it is added to the finished oil according to a certain dosage, it can still remain clear and transparent after standing for one year, while the oil prepared by the commercially available alkylated N-phenyl-α-naphthylamine will become turbid after standing for a period of time.
[0095] Commercially available alkylated N-phenyl-α-naphthylamine and the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in Examples 1 to 3 were added to base oil at the same dosage to prepare normal oil sample 1, normal oil sample 2, improved oil sample 1, improved oil sample 2 and improved oil sample 3. The high temperature oxidation resistance of the samples was tested according to ASTM D6186, "Standard Test Method for Oxidation Induction Time of Lubricating Oils by Pressure Differential Scanning Calorimetry (PDSC)". This test is conducted in an oxygen atmosphere by monitoring the oxidation process of the oil by detecting the heat released by the oil due to heating and oxidation. The oxidation resistance time can be obtained by analyzing the data. The longer the oxidation resistance time, the stronger the antioxidant capacity. The test results are shown in Table 3 below:
[0096] Table 3 High temperature antioxidant test results
[0097] Oil sample batch number Antioxidant time / min Ordinary oil sample 1 60.25 Ordinary oil sample 2 62.34 Improved oil sample 1 73.39 Improved oil sample 2 76.57 Improved oil sample 3 79.55
[0098] It can be seen from the above experimental results that the commercially available alkylated N-phenyl-α-naphthylamine and the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in this embodiment have good antioxidant effects. However, compared with the alkylated N-phenyl-α-naphthylamine additives sold on the market, the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in this embodiment have better antioxidant effects, which can improve the disadvantage of short service life of lubricating oil under high temperature conditions.
[0099] Thermogravimetric analysis was performed on the commercially available alkylated N-phenyl-α-naphthylamine and the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in Example 3. Figure 2 FIG. 1 is a schematic diagram of thermogravimetric analysis of the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative composition synthesized in Example 3. Figure 3The figure shows the thermogravimetric analysis of commercially available alkylated N-phenyl-α-naphthylamine. Thermogravimetric analysis is to evaluate the thermal stability of lubricating oil by measuring the relationship between the mass of the sample and the temperature (or time) under program temperature control. Generally speaking, the higher the initial decomposition temperature and the final decomposition temperature, the better the thermal stability. The test results are shown in Table 4 below:
[0100] Table 4 Thermal stability test results
[0101] Sample name Initial decomposition temperature / ℃ Final decomposition temperature / ℃ Mass loss / % Commercially available N-phenyl-α-naphthylamine 245.69 325.40 99.378 Example 3 Synthesis 277.17 339.73 99.605
[0102] It can be seen from the test results that the initial decomposition temperature and the final decomposition temperature of the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in this embodiment are significantly higher than those of the commercially available alkylated N-phenyl-α-naphthylamine, indicating that the N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine derivative compositions synthesized in this embodiment have better thermal stability.
[0103] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A liquid N-phenylnaphthylamine derivative high temperature antioxidant, It is characterized in that In terms of mass percentage, it includes: At least 98 wt% of a mixture of alkylated and arylated N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines, and less than 2 wt% of a mixture of unsubstituted N-phenyl-α-naphthylamines and N-phenyl-β-naphthylamines.
2. A method for preparing a liquid N-phenylnaphthylamine derivative high temperature antioxidant, It is characterized in that The method for preparing the liquid N-phenylnaphthylamine derivative high-temperature antioxidant according to claim 1 comprises: Adding N-phenyl-α-naphthylamine, a phosphoric acid / nitric acid modified halloysite catalyst and a polymerization inhibitor into a closed reactor, and removing moisture from the reactor; Adding olefin dropwise into the reaction kettle to carry out alkylation reaction; After adding N-phenyl-β-naphthylamine to the reaction kettle, olefin is added dropwise again; The acidic solid catalyst in the reactor is removed by filtration, and unreacted olefins are removed by reduced pressure distillation to obtain a liquid alkylated N-phenylnaphthylamine derivative high-temperature antioxidant.
3. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The preparation process of the phosphoric acid / nitric acid modified halloysite catalyst comprises: Halloysite is added into a mixed solution of phosphoric acid and nitric acid, heated under reflux at 70° C. for 12 hours, filtered, and the filter cake is dried at 100° C., ground and passed through a 300-mesh sieve to obtain a phosphoric acid / nitric acid modified halloysite catalyst; The mass fraction ratio of phosphoric acid to nitric acid is 1:1, and the total concentration of phosphoric acid and nitric acid is 10-30wt%; Wherein, the addition amount of the phosphoric acid / nitric acid modified halloysite catalyst is 5% to 30% of the total mass of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine.
4. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The polymerization inhibitor includes hydroquinone, tert-butyl catechol, 2,6-dinitro-p-cresol and 2,5-di-tert-amylhydroquinone, and the addition amount of the polymerization inhibitor is 30-150 ppm.
5. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The olefin is selected from tripropylene, tetrapropylene or styrene, and the olefin is added all at once or in batches for multiple times, and the styrene accounts for 0 to 10% of the total molar amount of the olefin; The molar ratio of the total amount of the olefin added to the total amount of N-phenyl-α-naphthylamine and N-phenyl-β-naphthylamine is 2.5:1 to 6:
1.
6. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The N-phenyl-β-naphthylamine accounts for 0 to 20% of the total molar amount of the N-phenyl-α-naphthylamine and the N-phenyl-β-naphthylamine.
7. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The filter cake is collected and processed and then recycled as a catalyst, and the olefin removed by vacuum distillation is recycled as a raw material to participate in the reaction.
8. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that The specific operation of removing the water in the reactor includes: Using nitrogen to replace the air in the closed reactor; The reactor was heated until the temperature reached 70° C., and the stirring and vacuum systems of the reactor were turned on; When the temperature rises to 100° C., the temperature is kept for half an hour to remove the moisture in the reactor; The vacuum system was stopped, and the reactor was replaced with nitrogen to a normal pressure state.
9. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that During the alkylation reaction, the olefin is added dropwise within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.
10. The method for preparing the liquid N-phenylnaphthylamine derivative high temperature antioxidant according to claim 2, It is characterized in that After adding N-phenyl-β-naphthylamine into the reaction kettle, the olefin is added dropwise again within 30 minutes, while the reaction temperature is maintained at 110° C. to 210° C., and the reaction time is 6 to 24 hours.