Heat treatment process of high-toughness welding wire steel
Through multi-stage heat treatment process and cleaning treatment, the problem of single heat treatment process of high-strength tough welded wire steel is solved, the mechanical properties and processing properties of welded wire steel are improved, and the welding quality is ensured.
Patent Information
- Application Number
- CN202411013307.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high-strength tough wire steel has a single heat treatment process, which leads to insufficient mechanical properties such as bending strength and tensile strength of welding wire steel, and does not have good hardness and toughness. The mechanical properties need to be improved and the processing performance is not good, which affects the welding quality. and effects.
A multi-stage heat treatment process is adopted, including two heating and cooling of the resistor furnace and induction furnace, combined with the composite coolant treatment in the vacuum furnace, and the mechanical properties and processing properties of the welding wire steel are improved through the cleaning treatment of acidic and alkaline solutions.
The bending strength, tensile strength, hardness and toughness of welding wire steel are significantly improved, mechanical properties are improved, subsequent processing process is simplified, and welding quality and effect are ensured.
Smart Images

Figure CN118957243A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding wire steel processing, and in particular to a heat treatment process for high-strength and toughness welding wire steel. Background Art
[0002] Welding wire steel is a metal wire material used for welding. It mainly plays the role of filler metal in the welding process and also serves as a conductive electrode. There are many types of welding wire steel. According to different classification standards, it can be divided into solid welding wire and flux-cored welding wire. Solid welding wire is made of hot-rolled wire by drawing. In order to prevent the welding wire from rusting, the surface of the welding wire must be specially treated. At present, it is mainly copper plating. Flux-cored welding wire is a welding wire made by wrapping powder in a thin steel strip and rolling it into different cross-sectional shapes through rolling and drawing. It is also called powder-cored welding wire, tubular welding wire or folded welding wire.
[0003] High-strength and toughness welding wire steel refers to a welding wire material used for welding steels with high strength and high toughness requirements. During the processing of high-strength and toughness welding wire steel, the welding wire steel generally needs to be heat treated. The purpose of heat treatment of welding wire steel is mainly to improve its mechanical properties, eliminate internal stress, refine grains, improve toughness and plasticity, and adjust its chemical composition and organizational structure, so as to achieve the effect of improving the quality and performance of the welded joint.
[0004] Most of the existing heat treatment processes for high-strength and toughness welding wire steels have a single process, and only achieve heat treatment of the welding wire steel through simple quenching and quenching, resulting in the welding wire steel after heat treatment being insufficient in mechanical properties such as bending strength and tensile strength, and not having good hardness and toughness, and the mechanical properties need to be improved. In addition, the processing performance is not good, which not only brings difficulties to the subsequent welding wire processing, but also causes the subsequent processed welding wire performance to be deficient, and cannot guarantee good welding quality and effect. Therefore, the present invention proposes a heat treatment process for high-strength and toughness welding wire steel to solve the problems existing in the prior art. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to propose a heat treatment process for high-strength and toughness welding wire steel to solve the problems that the existing heat treatment process flow of high-strength and toughness welding wire steel is single, the heat-treated welding wire steel is insufficient in mechanical properties such as bending strength and tensile strength, and does not have good hardness and toughness, the mechanical properties need to be improved, and the processing performance is also poor.
[0006] In order to achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a heat treatment process of high-strength and tough welding wire steel, comprising the following steps:
[0007] Step 1: First, clean the surface of the welding wire steel to be processed, and then preheat the welding wire steel with a resistance heater after cleaning;
[0008] Step 2: Place the preheated welding wire steel in a resistance furnace and heat it to 870-880°C, then keep it warm. After keeping warm for a preset time, turn off the resistance furnace and cool the welding wire steel in the furnace to room temperature. Then place the welding wire steel in an induction furnace and heat it to 860-875°C by the induction furnace. Then take the welding wire steel out of the induction furnace and let it cool naturally in the air to room temperature to complete the primary heat treatment.
[0009] Step 3: prepare a composite coolant in advance, then place the welding wire steel that has undergone the primary heat treatment in step 1 into a vacuum furnace and heat it to 830-845°C and keep it warm, then take out the welding wire steel that has been kept warm and place it into the composite coolant to cool it, wipe the surface of the welding wire steel after cooling to room temperature, then place it in the vacuum furnace again and heat it to 225-275°C and keep it warm, take out the welding wire steel after keeping it warm for a preset time and cool it to room temperature, and complete the secondary heat treatment;
[0010] Step 4: firstly pickle the welding wire steel after the secondary heat treatment with an acid solution, then pickle the welding wire steel with an alkaline solution, then rinse the welding wire steel with deionized water, and then dry it after rinsing to obtain high-strength and tough welding wire steel.
[0011] A further improvement is that in step one, the specific steps for surface cleaning of the welding wire steel are: first, the surface of the welding wire steel is sandblasted using a sandblasting machine, then the surface of the welding wire steel is cleaned using a high-pressure water flow, then the surface of the welding wire steel is placed in an ultrasonic cleaning machine for ultrasonic cleaning, and finally, it is dried using a vacuum dryer.
[0012] A further improvement is that in the step 1, the welding wire steel is preheated at a heating rate of 10 to 15°C / min, and the preheating is completed after the preheating reaches 200 to 300°C.
[0013] A further improvement is that in the step 2, the welding wire steel is heated to 870-880°C in a resistance furnace at a heating rate of 25-35°C / min, the welding wire steel is kept warm in the resistance furnace for 45-60 minutes after being heated to 870-880°C, and then the resistance furnace is closed and cooling begins, and the welding wire steel is heated to 860-875°C in an induction furnace at a heating rate of 25-30°C / min.
[0014] A further improvement is that in step three, the composite coolant is prepared by mixing water, sodium chloride, a polymer additive, a rust inhibitor and a defoamer in a mass ratio of 25:2:4:1:1, the polymer additive is selected from one of polyvinyl alcohol or polyacrylamide, the rust inhibitor is selected from one of phosphate or borate, and the defoamer is selected from one of soybean oil or castor oil.
[0015] A further improvement is that in the step three, the welding wire steel is heated to 830-845°C in a vacuum furnace at a heating rate of 35-45°C / min, and the welding wire steel is kept warm for 30-45 minutes after being heated to 830-845°C.
[0016] A further improvement is that in the step three, the welding wire steel is heated to 225-275°C in a vacuum furnace at a heating rate of 40-50°C / min, and the welding wire steel is kept warm for 10-20 minutes after being heated to 225-275°C.
[0017] A further improvement is that in the step 4, the acidic solution is selected from one of a nitric acid solution or a phosphoric acid solution, the alkaline solution is selected from one of a sodium hydroxide solution or a potassium hydroxide solution, and the welding wire steel is dried with a hot air blower after rinsing.
[0018] The beneficial effects of the present invention are as follows: the present invention realizes the primary heat treatment by heating and cooling the welding wire steel twice in the resistance furnace and the induction furnace respectively, which can improve the plasticity of the welding wire steel to a certain extent, eliminate its internal stress, facilitate subsequent processing into welding wire, and improve the mechanical properties of the material; and realizes the secondary heat treatment by heating and cooling the welding wire steel twice in the vacuum furnace, which can make the welding wire steel quickly cooled after austenitization, improve the hardness and strength, and reduce the internal stress caused by multiple heating treatments, and further adjust the mechanical properties of the welding wire steel. The welding wire steel subjected to the above-mentioned heat treatment process has good bending strength, tensile strength, hardness and toughness, and the mechanical properties are significantly improved. At the same time, the processing performance of the welding wire steel is improved, which brings convenience to the subsequent welding wire processing, ensures the welding wire performance, and ensures the welding quality and effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 It is a schematic flow diagram of the heat treatment process of the high-strength and toughness welding wire steel of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The chemical composition of the welding wire steel used in the present invention is as follows by weight: C: 0.10%, Si: 0.04%, Mn: 0.60%, As: 0.007%, Al: 0.015%, Sn: 0.015%, N: 0.01%, Ti: 0.20%, O: 0.002%, and the balance is iron.
[0023] Embodiment 1
[0024] See also Figure 1 This embodiment provides a heat treatment process for high-strength and tough welding wire steel, comprising the following steps:
[0025] Step 1: Clean and preheat before heat treatment
[0026] First, the surface of the welding wire steel is sandblasted with a sandblasting machine to remove rust, scale and other attachments on the steel surface. Then, the surface of the welding wire steel is cleaned with a high-pressure water flow to remove loose dirt and residues. Then, it is placed in an ultrasonic cleaning machine for ultrasonic cleaning. The cavitation effect of ultrasound in the liquid is used to remove tiny particles and difficult-to-remove dirt on the surface of the steel. Finally, a vacuum dryer is used to dry it to prevent impurities on the surface of the welding wire steel from affecting the subsequent heat treatment effect. After cleaning, a resistance heater is used to preheat the welding wire steel to 200°C at a heating rate of 10°C / min.
[0027] Step 2: Initial heat treatment
[0028] The preheated welding wire steel is placed in a resistance furnace and heated to 870°C at a heating rate of 25°C / min, and then kept warm. After keeping warm for 45 minutes, the resistance furnace is turned off and the welding wire steel is placed in the furnace to slowly cool to room temperature. Then the welding wire steel is placed in an induction furnace, and the welding wire steel is heated to 860°C at a heating rate of 25°C / min by the induction furnace. Then the welding wire steel is taken out of the induction furnace and placed in the air to naturally cool to room temperature to complete the initial heat treatment. Through two heating and cooling treatments, the plasticity of the welding wire steel can be improved to a certain extent, its internal stress can be eliminated, and it is convenient for subsequent processing into welding wire, and the mechanical properties of the material are improved, the grains are refined, and it is helpful to improve the strength of the welding wire steel;
[0029] Step 3: Secondary heat treatment
[0030] A composite coolant is prepared in advance, and the welding wire steel that has undergone the primary heat treatment in step one is placed in a vacuum furnace and heated to 830°C at a heating rate of 35°C / min and kept warm for 30 minutes to austenitize it. Then, the welding wire steel that has been kept warm is taken out and placed in the composite coolant for cooling. After cooling to room temperature, the surface of the welding wire steel is wiped clean, and then it is placed in the vacuum furnace again and heated to 225°C at a heating rate of 40°C / min and kept warm. After keeping warm for 10 minutes, the welding wire steel is taken out and cooled to room temperature to complete the secondary heat treatment. By heating and cooling the welding wire steel twice in the vacuum furnace, and cooling the welding wire steel with the pre-prepared composite coolant after the first heating, the welding wire steel can be quickly cooled after austenitization, thereby improving hardness and strength, while reducing internal stress caused by multiple heating treatments, further adjusting the mechanical properties of the welding wire steel, and improving toughness and stability;
[0031] The composite coolant of the present embodiment is prepared by mixing water, sodium chloride, polymer additive, rust inhibitor and defoamer in a mass ratio of 25:2:4:1:1. The composite coolant prepared by the above raw materials is more efficient and has better effect than traditional water cooling and brine cooling. The polymer additive is polyvinyl alcohol, the rust inhibitor is phosphate, which plays a rust-proof role, and the defoamer is soybean oil, which is environmentally friendly and pollution-free.
[0032] Step 4: Cleaning and deoxidation after heat treatment
[0033] First, the welding wire steel that has undergone secondary heat treatment is pickled with an acid solution to remove surface oxides and residual cooling medium, and then the pickled welding wire steel is alkali-washed with an alkaline solution to neutralize the acidic substances remaining on the surface of the welding wire steel and further clean the surface, and then the welding wire steel is rinsed with deionized water. After rinsing, it is dried with a hot air blower to obtain high-strength and tough welding wire steel. Through the above cleaning treatment, the surface of the welding wire steel is cleaner, which is convenient for subsequent processing into welding wire;
[0034] The acidic solution in this embodiment is a 1M nitric acid solution, and the alkaline solution is a 1M sodium hydroxide solution.
[0035] Embodiment 2
[0036] See also Figure 1 This embodiment provides a heat treatment process for high-strength and tough welding wire steel, comprising the following steps:
[0037] Step 1: Clean and preheat before heat treatment
[0038] First, the surface of the welding wire steel is sandblasted with a sandblasting machine to remove rust, scale and other attachments on the steel surface. Then, the surface of the welding wire steel is cleaned with a high-pressure water flow to remove loose dirt and residues. Then, it is placed in an ultrasonic cleaning machine for ultrasonic cleaning. The cavitation effect of ultrasound in the liquid is used to remove tiny particles and difficult-to-remove dirt on the surface of the steel. Finally, a vacuum dryer is used to dry it to prevent impurities on the surface of the welding wire steel from affecting the subsequent heat treatment effect. After cleaning, a resistance heater is used to preheat the welding wire steel to 300°C at a heating rate of 15°C / min.
[0039] Step 2: Initial heat treatment
[0040] The preheated welding wire steel is placed in a resistance furnace and heated to 880°C at a heating rate of 35°C / min, and then kept warm. After keeping warm for 60 minutes, the resistance furnace is turned off and the welding wire steel is placed in the furnace to slowly cool to room temperature. Then the welding wire steel is placed in an induction furnace, and the welding wire steel is heated to 875°C at a heating rate of 30°C / min by the induction furnace. Then the welding wire steel is taken out of the induction furnace and placed in the air to naturally cool to room temperature to complete the initial heat treatment. Through two heating and cooling treatments, the plasticity of the welding wire steel can be improved to a certain extent, its internal stress can be eliminated, and it is convenient for subsequent processing into welding wire, and the mechanical properties of the material are improved, the grains are refined, and it is helpful to improve the strength of the welding wire steel;
[0041] Step 3: Secondary heat treatment
[0042] A composite coolant is prepared in advance, and the welding wire steel that has undergone the primary heat treatment in step one is placed in a vacuum furnace and heated to 845°C at a heating rate of 45°C / min and kept warm for 45 minutes to austenitize it. Then, the welding wire steel that has been kept warm is taken out and placed in the composite coolant for cooling. After cooling to room temperature, the surface of the welding wire steel is wiped clean, and then it is placed in the vacuum furnace again and heated to 275°C at a heating rate of 50°C / min and kept warm. After keeping warm for 20 minutes, the welding wire steel is taken out and cooled to room temperature to complete the secondary heat treatment. By heating and cooling the welding wire steel twice in the vacuum furnace, and cooling the welding wire steel with the pre-prepared composite coolant after the first heating, the welding wire steel can be quickly cooled after austenitization, thereby improving hardness and strength, while reducing internal stress caused by multiple heating treatments, further adjusting the mechanical properties of the welding wire steel, and improving toughness and stability;
[0043] The composite coolant of the present embodiment is prepared by mixing water, sodium chloride, polymer additive, rust inhibitor and defoamer in a mass ratio of 25:2:4:1:1. The composite coolant prepared by the above raw materials is more efficient and has better effect than traditional water cooling and brine cooling. The polymer additive is polyacrylamide, the rust inhibitor is borate, which plays a rust-proof role, and the defoamer is castor oil, which is environmentally friendly and pollution-free.
[0044] Step 4: Cleaning and deoxidation after heat treatment
[0045] First, the welding wire steel that has undergone secondary heat treatment is pickled with an acid solution to remove surface oxides and residual cooling medium, and then the pickled welding wire steel is alkali-washed with an alkaline solution to neutralize the acidic substances remaining on the surface of the welding wire steel and further clean the surface, and then the welding wire steel is rinsed with deionized water. After rinsing, it is dried with a hot air blower to obtain high-strength and tough welding wire steel. Through the above cleaning treatment, the surface of the welding wire steel is cleaner, which is convenient for subsequent processing into welding wire;
[0046] In this embodiment, the acidic solution is a 1M phosphoric acid solution, the alkaline solution is a 1M potassium hydroxide solution, and the reducing agent is a 1M sulfite solution.
[0047] The high-strength and tough welding wire steel obtained by heat treatment in Example 1 and Example 2 of the present invention was analyzed for mechanical properties after heat treatment, and the existing welding wire steel (purchased on the market with the same composition) after annealing and quenching heat treatment was tested as a comparative example (wherein the yield strength test standard refers to GB / T 228.1-2010, the tensile strength test standard refers to GB / T228.1-2010, the hardness test standard refers to GB / T 231.1-2009, the impact toughness test standard refers to GB / T 229-2020, and the wear test standard refers to GB / T 12444-2006). The test results are shown in Table 1 below:
[0048] Table 1 Test results
[0049]
[0050] It can be seen from Table 1 above that the high-strength and toughness welding wire steel obtained by heat treatment in Example 1 and Example 2 of the present invention is significantly superior to the welding wire steel subjected to annealing and quenching heat treatment in terms of mechanical properties such as yield strength, tensile strength, hardness, impact toughness and wear resistance.
[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A heat treatment process for high-strength and tough welding wire steel, characterized in that: The following steps are involved: Step 1: First, clean the surface of the welding wire steel to be processed, and then preheat the welding wire steel with a resistance heater after cleaning; Step 2: Place the preheated welding wire steel in a resistance furnace and heat it to 870-880°C, then keep it warm. After keeping warm for a preset time, turn off the resistance furnace and cool the welding wire steel in the furnace to room temperature. Then place the welding wire steel in an induction furnace and heat it to 860-875°C by the induction furnace. Then take the welding wire steel out of the induction furnace and let it cool naturally in the air to room temperature to complete the primary heat treatment. Step 3: prepare a composite coolant in advance, then place the welding wire steel that has undergone the primary heat treatment in step 1 into a vacuum furnace and heat it to 830-845°C and keep it warm, then take out the welding wire steel that has been kept warm and place it into the composite coolant to cool it, wipe the surface of the welding wire steel after cooling to room temperature, then place it in the vacuum furnace again and heat it to 225-275°C and keep it warm, take out the welding wire steel after keeping it warm for a preset time and cool it to room temperature, and complete the secondary heat treatment; Step 4: firstly pickle the welding wire steel after the secondary heat treatment with an acid solution, then pickle the welding wire steel with an alkaline solution, then rinse the welding wire steel with deionized water, and then dry it after rinsing to obtain high-strength and tough welding wire steel.
2. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step 1, the specific steps of surface cleaning the welding wire steel are: firstly, the surface of the welding wire steel is sandblasted by a sandblasting machine, then the surface of the welding wire steel is cleaned by a high-pressure water flow, then the surface of the welding wire steel is placed in an ultrasonic cleaning machine for ultrasonic cleaning, and finally, the surface of the welding wire steel is dried by a vacuum dryer.
3. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step 1, the welding wire steel is preheated at a heating rate of 10 to 15°C / min, and the preheating is completed after the preheating reaches 200 to 300°C.
4. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step 2, the welding wire steel is heated to 870-880°C in a resistance furnace at a heating rate of 25-35°C / min. After being heated to 870-880°C, the welding wire steel is kept warm in the resistance furnace for 45-60 minutes, and then the resistance furnace is closed and cooling begins. The welding wire steel is heated to 860-875°C in an induction furnace at a heating rate of 25-30°C / min.
5. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step three, the composite coolant is prepared by mixing water, sodium chloride, a polymer additive, a rust inhibitor and a defoamer in a mass ratio of 25:2:4:1:1, the polymer additive is selected from one of polyvinyl alcohol or polyacrylamide, the rust inhibitor is selected from one of phosphate or borate, and the defoamer is selected from one of soybean oil or castor oil.
6. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step three, the welding wire steel is heated to 830-845° C. at a heating rate of 35-45° C. / min in a vacuum furnace, and the welding wire steel is kept warm for 30-45 minutes after being heated to 830-845° C.
7. The heat treatment process of high-strength and tough welding wire steel according to claim 1, characterized in that: In the step three, the welding wire steel is heated to 225-275° C. at a heating rate of 40-50° C. / min in a vacuum furnace, and the welding wire steel is kept warm for 10-20 minutes after being heated to 225-275° C.
8. The heat treatment process of a high-strength and tough welding wire steel according to claim 1, characterized in that: In the step 4, the acidic solution is selected from one of a nitric acid solution or a phosphoric acid solution, the alkaline solution is selected from one of a sodium hydroxide solution or a potassium hydroxide solution, and the welding wire steel is dried by a hot air blower after rinsing.