Preparation method of novel graphitized polypyrrole sphere reinforced copper-based composite material
Through molecular-level mixing method and rapid hot pressing sintering technology, the stable synthesis and uniform dispersion of graphitized polypyrrole balls in copper-based composite materials are solved, and the copper-based composite materials with high strength and conductivity are realized, which improves the material comprehensive performance.
Patent Information
- Application Number
- CN202411060140.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The existing copper-based composite materials have poor mechanical properties, low conductivity, and are difficult to stably synthesize and uniformly disperse graphitized polypyrrole spheres (G-PNSs) reinforced phases, which hinders the research on the new graphitized polypyrrole sphere reinforced copper-based composite materials. Progress and application.
Using molecular-level mixing method (MLM) and rapid hot pressing sintering technology, the chemical bridging reaction between graphitized polypyrrole nanospheres (G-PNSs) and copper matrix is optimized to combine the interface to form a G- with corrugated structure and strong roughness. PNSs/Cu composite powder, and a high-performance G-PNSs/Cu composite material was obtained by sintering.
The high strength of the material, improved plasticity and toughness, optimized processing performance, improved the breaking strength and conductivity of the material, and obtained a copper-based composite material with high comprehensive performance.
Smart Images

Figure CN118957338A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material. Background Art
[0002] Copper has excellent electrical and thermal conductivity and ductility, and is widely used in power transmission cables, tram contact switches, brushes, integrated circuit leads and other fields. Polypyrrole (PPy), as a conductive polymer, has good conductivity advantages. Since the discovery of PPy, it has attracted widespread attention in the field of nanomaterials due to its excellent mechanical and physicochemical properties. Polypyrrole nanospheres (PNSs) are an outstanding representative of PPy. After high-temperature graphitization, they become a carbon nanomaterial rich in carbon and nitrogen - graphitized polypyrrole spheres (G-PNSs). At present, most copper-based composites are tubular or low-dimensional carbon nanophase reinforced copper-based composites. Their preparation methods are relatively traditional, and the resulting composites have poor mechanical properties and low electrical conductivity. The rich nitrogen element in G-PNSs can regulate the electronic structure, which is beneficial to the improvement of electrical conductivity. In addition, from the perspective of mechanical strengthening, regulating the dispersion distribution of G-PNSs in the copper matrix crystal can effectively enhance the fracture strength of the material by pinning dislocation slip and increasing the dislocation storage density. Therefore, the use of G-PNSs as a reinforcing phase provides a new opportunity for the development of high-strength and high-conductivity copper-based composites.
[0003] However, there are still great difficulties in how to stably synthesize G-PNSs, achieve uniform dispersion of the reinforcing phase, and efficiently exert the intrinsic strengthening effect of the reinforcement, which hinders the research progress and application of new graphitized polypyrrole ball reinforced copper-based composites. Summary of the invention
[0004] Based on the above research background, the present invention proposes a method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material. On the one hand, the preparation method can refine the grains, improve the strength of the material, improve the plasticity and toughness, and optimize the processing performance and appearance quality of the material, while also promoting the uniform dispersion of G-PNSs in the copper matrix; on the other hand, through molecular level mixing, the chemical bridging effect of the self-contained elements in G-PNSs can improve the wettability between G-PNSs and the copper matrix and strengthen the interface bonding of G-PNSs. Finally, the prepared G-PNSs exhibited obvious corrugated structure and strong roughness on its side wall, and further pinned dislocation slip, effectively enhancing the fracture strength of the material. Therefore, the prepared copper-based composite material can maintain good conductivity while obtaining excellent mechanical properties, realizing the successful development of high-comprehensive performance copper-based composite materials.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material, the steps of which are as follows:
[0007] (1) Preparation of graphitized polypyrrole nanospheres (G-PNSs) reinforcement
[0008] Weigh 1g to 3g of FeCl3·6H2O (99%) brown-yellow powder into a 500ml beaker, then add 100ml deionized water for ultrasonic dispersion for 10min to 20min. After the ultrasonication is completed, place it on a magnetic stirrer for stirring. Subsequently, use a pipette to extract 420μL of pyrrole (98%) and slowly drip it into the FeCl3·6H2O solution, and stir it at room temperature for 24h. After that, functional PNSs powder is obtained by filtration and vacuum drying. Then, inert gas is introduced into a vacuum tube furnace for graphitization at 650℃ to 1000℃ to obtain G-PNSs powder.
[0009] (2) Preparation of G-PNSs / Cu composite powder
[0010] Weigh appropriate amounts of G-PNSs powder and CuAc·H2O and perform ultrasonic dispersion respectively, then add the G-PNSs dispersion solution into the CuAc·H2O solution and stir in a water bath to obtain a G-PNSs / CuAc mixed solution, then add sodium hydroxide and glucose solution in sequence, stir, filter, dry and reduce to obtain a G-PNSs / Cu2O composite powder;
[0011] Further optimization, the specific operation of step (2) is as follows: weigh 0.3g to 3g of graphitized polypyrrole sphere (G-PNSs) powder and 15g to 150g of hydrated copper acetate (CuAc·H2O) and ultrasonically disperse them in deionized water for 10min to 20min respectively for later use, add the G-PNSs dispersion solution to the CuAc·H2O solution, and stir for 30min to 60min in a water bath environment at 60℃ to 80℃ to obtain a G-PNSs / CuAc mixed solution. Subsequently, weigh 9g to 90g of sodium hydroxide (0.5mol / L) and 7g to 70g of glucose (0.8mol / L) and disperse them into a solution and then add the above mixed solution in sequence, stop stirring when the color of the solution changes from dark blue to brick red, and obtain G-PNSs / Cu2O powder by filtering and vacuum drying. Finally, the above powder is reduced in a vacuum tube furnace with Ar / H2 as protective reducing gas at a certain temperature for a period of time to obtain G-PNSs / Cu composite powder. The reaction principle is shown in (1)(2)(3)(4):
[0012] Cu(Ac)2·H2O + 2NaOH → Cu(OH)2↓ + 2NaAc+ H2O (1)
[0013] Cu(OH)2 → CuO↓ + H2O (2)
[0014] 2CuO + C6H 12 O6 + NaOH → Cu2O↓ + C6H 11 O7Na + H2O (3)
[0015] Cu2O + H2 → 2Cu + H2O (4)
[0016] (3) Preparation of G-PNSs / Cu composite closed-cell powder
[0017] The G-PNSs / Cu powder with holes obtained in step (2) is placed in a ball mill, alcohol is added, and argon is used as a protective gas. After ball milling for 120 minutes to 180 minutes, the powder is vacuum dried to obtain a G-PNSs / Cu flaky composite powder. The flaky powder has a large specific surface area and can effectively improve the interface bonding between G-PNSs and the copper substrate.
[0018] (4) Preparation of G-PNSs / Cu composites
[0019] Weigh 30 g to 300 g of the G-PNSs / Cu composite powder obtained in step (3), evacuate the furnace body to vacuum (with Ar as protective gas) in a fast hot pressing sintering furnace (FHP), and sinter at 600° C. to 700° C. After keeping warm for 10 min to 15 min, turn off the vacuum, turn off the instrument, and take out the sample after the furnace cools to room temperature (about 20 min) to obtain a G-PNSs / Cu composite block.
[0020] Preferably, in the step (1), the proportion of G-PNSs powder is: 0.1wt% to 0.2wt% (calculated based on the total amount); the particle size is 100nm to 200nm; and the morphology is spherical particles.
[0021] Preferably, in step (2), CuAc·H2O is of analytical grade (AR≥99%); NaOH is of analytical grade (AR≥99%); and glucose is of analytical grade (AR≥99%).
[0022] Preferably, the vacuum drying in step (1) adopts a vacuum rotary evaporation device, and the rotation speed thereof is ≤50r / min.
[0023] Preferably, in step (2), the vacuum tube furnace has a heating rate of 5°C / min to 10°C / min, a holding temperature of 300°C to 400°C, and a holding time of 200min to 300min.
[0024] Preferably, in step (3), the amount of alcohol added is 1 / 4 to 1 / 3 of the volume of the ball mill; the ball-to-material ratio is 10:1 to 15:1; the ball milling time is 120 min to 180 min; and the ball milling speed is 200 r / min to 250 r / min.
[0025] Preferably, in step (3), the particle size of the G-PNSs / Cu composite powder is 20 μm to 50 μm; the morphology is spherical or flaky, or any irregular shape.
[0026] Preferably, in step (4), the initial vacuum degree of the rapid hot pressing sintering furnace is: 5×10 -4 ~10 -3 Pa; heating rate: 50℃ / min~100℃ / min, sintering temperature is 600℃~700℃; holding time is 10min~15min.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention proposes a method for stably preparing a graphitized polypyrrole ball reinforced copper-based composite material. On the one hand, the MLM method for preparing G-PNSs / Cu composite powder can refine the grains, improve the strength of the material, improve the plasticity and toughness, and optimize the processing performance and appearance quality of the material, while also promoting the uniform dispersion of G-PNSs in the copper matrix; on the other hand, the rapid hot pressing sintering technology (FHP) can improve the interface bonding between the copper matrix and G-PNSs, thereby ensuring and improving the performance of the composite material.
[0029] (2) Compared with traditional tubular or low-dimensional carbon nanophase reinforced copper-based composites, the G-PNSs prepared by the present invention exhibits obvious corrugated structure and strong roughness on its side wall. The fracture strength of the material is effectively enhanced by pinning dislocation slip and increasing the dislocation storage density, so that the G-PNSs / Cu composite material has excellent mechanical properties and good electrical conductivity, thus realizing the successful development of high-comprehensive performance copper-based composite materials.
[0030] (3) The preparation method of the present invention has a short cycle and strong practicality, and provides technical guidance for the research and development of high-performance copper-based composite materials for application in the field of power electronic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced and explained below.
[0032] Figure 1 This is a transmission electron microscopy (TEM) image of the G-PNSs powder in step (1) of Example 1;
[0033] Figure 2 This is a scanning electron microscope image (SEM) of the G-PNSs / Cu powder after ball milling in step (2) of Example 1;
[0034] Figure 3 The conductivity and hardness change bar graph of the 0.15% G-PNSs / Cu composite material and the pure Cu material in Example 3 and Comparative Example 3;
[0035] Figure 4 The stress-strain curves of the 0.15% G-PNSs / Cu composite material and the pure Cu material in Example 3 and Comparative Example 3;
[0036] Figure 5 The conductivity and hardness change bar graph of 0.1% G-PNSs / Cu composite material and pure Cu material in Example 1 and Comparative Example 1;
[0037] Figure 6 1 and 2 are stress-strain curves of 0.1% G-PNSs / Cu composite material and pure Cu material in Example 1 and Comparative Example 1.
[0038] Figure 7 The bar graphs of conductivity and hardness changes of 0.2% G-PNSs / Cu composite material and pure Cu material in Example 2 and Comparative Example 2 are shown;
[0039] Figure 8 These are the stress-strain curves of the 0.2% G-PNSs / Cu composite material and pure Cu material in Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0041] In the following embodiments:
[0042] The purity of G-PNSs powder is 99.9%, and the diameter is 100nm-200nm; the proportion of G-PNSs powder is 0.1wt%-0.2wt% (calculated by total amount); homemade;
[0043] CuAc·H2O, NaOH, and glucose were all analytical grade (AR ≥ 99%) and were obtained from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0044] The purity of Cu powder is 99.9%, the particle size is 20μm to 50μm, and the morphology can be spherical, flake, or any irregular shape. Shanghai Naio Nano Technology Co., Ltd.
[0045] Scanning electron microscope: Nova Nano-450, FEI, USA;
[0046] Transmission electron microscope: SA 58000x, FEI, USA;
[0047] Mechanical properties of the G-PNSs / Cu composites prepared in the examples and comparative examples were characterized by using a universal tensile testing machine (AUTOGRAPH AG-I, Shimadzu Corporation, Japan) to perform tensile tests at room temperature, wherein the sample size (dog bone type) was 16 mm × 2 mm × 1.5 mm (length × width × thickness); the tensile rate was 0.2 mm / min.
[0048] Example 1
[0049] A novel method for preparing a graphitized polypyrrole ball reinforced copper-based composite material, wherein polypyrrole nanospheres (PNSs) are first prepared by chemical synthesis, and then graphitized polypyrrole balls (G-PNSs) are obtained as reinforcements by graphitization. G-PNSs / Cu composite powders are obtained by molecular-level blending (MLM) combined with low-energy ball milling "closed-cell" technology. The above powders are subjected to rapid hot pressing (FHP) to obtain G-PNSs / Cu composite materials.
[0050] The specific steps are as follows:
[0051] (1) Preparation of graphitized polypyrrole nanospheres (G-PNSs) reinforcement
[0052] Weigh 1g of FeCl3·6H2O (99%) brown-yellow powder into a 500ml beaker, then add 100ml of deionized water for ultrasonic dispersion for 10 minutes. After the ultrasonication is completed, place it on a magnetic stirrer for stirring for later use. Subsequently, use a pipette to extract 420μL of pyrrole (98%) and slowly drip it into the FeCl3·6H2O solution, and stir it at room temperature for 24h. After that, functional PNSs powder is obtained by filtration and vacuum drying. After that, inert gas is introduced into a vacuum tube furnace for graphitization at 650°C to obtain spherical particle G-PNSs powder with a particle size of 100nm. The morphology is as follows Figure 1 shown.
[0053] (2) Preparation of G-PNSs / Cu composite powder
[0054] The graphitized polypyrrole ball (G-PNSs) powder obtained in step (1) was weighed 0.3g and 15g of hydrated copper acetate (CuAc·H2O) and ultrasonically dispersed in deionized water for 10min for later use. The G-PNSs dispersion solution was added to the CuAc·H2O solution and stirred in a 60°C water bath environment for 30min to obtain a G-PNSs / CuAc mixed solution. Subsequently, 9g of sodium hydroxide (0.5mol / L) and 7g of glucose (0.8mol / L) were weighed and dispersed into a solution and then added to the above mixed solution in sequence. When the color of the solution changed from dark blue to brick red, stirring was stopped, and G-PNSs / Cu2O powder was obtained by filtration and vacuum drying. Finally, the above powder was reduced at 300°C for 200min in a vacuum tube furnace with Ar / H2 as protective reducing gas at a heating rate of 5°C / min to obtain a G-PNSs / Cu composite powder.
[0055] (3) Preparation of G-PNSs / Cu composite closed-cell powder
[0056] The G-PNSs / Cu powder with holes obtained in step (2) was placed in a ball mill, and 1 / 4 of the volume of the ball mill was added with alcohol, and argon was used as the protective gas. After ball milling at a speed of 200 r / min for 120 min, the powder was vacuum dried to obtain a G-PNSs / Cu flaky composite powder. The flaky powder has a large specific surface area and can effectively improve the interface bonding between G-PNSs and the copper matrix. The morphology is as follows: Figure 2 shown.
[0057] (4) Preparation of G-PNSs / Cu composites
[0058] Weigh 30 g of the G-PNSs / Cu composite powder obtained in step (3) and evacuate the furnace body to vacuum (with Ar as protective gas) in a fast hot pressing sintering furnace (FHP), sinter at 600°C, keep warm for 10 minutes, turn off the vacuum, turn off the instrument, and take out the sample after the furnace cools to room temperature (about 20 minutes) to obtain a G-PNSs / Cu composite material.
[0059] Comparative Example 1
[0060] Weigh 30 g of Cu powder prepared by the MLM method, evacuate the furnace body into a vacuum (with Ar as the protective gas) in a fast hot pressing sintering furnace (FHP), and sinter at 600°C. After keeping warm for 10 minutes, turn off the vacuum and the instrument. After the furnace cools to room temperature (about 20 minutes), take out the sample to obtain a pure Cu block.
[0061] The conductivity and hardness of the composite materials prepared in Example 1 and Comparative Example 1 were tested. The results are as follows: Figure 5 As shown; for mechanical properties test, the results are as follows Figure 6 shown.
[0062] like Figure 5 As shown, the composite material obtained by the molecular-level blending method combined with the rapid hot pressing sintering process has better performance. Comparing Example 1 and Comparative Example 1, the composite material of Example 1 still maintains good electrical conductivity (about 99% IACS). As for hardness, the composite material of Example 1 has a significant improvement over the material of Comparative Example 1, from 78HV to 108HV, an increase of about 38.5%. The main reasons for this phenomenon are: on the one hand, Example 1 obtains uniformly dispersed G-PNSs particles through the MLM method; on the other hand, the chemical bridging reaction occurring in the MLM method in Example 1 and the pinning effect produced by the obvious corrugated structure on the side wall of G-PNSs effectively improve the interface bonding between G-PNSs and the copper matrix. However, the control group did not add reinforcement, resulting in lower performance than Example 1.
[0063] like Figure 6 As shown, the tensile strength of the composite material of Example 1 is significantly improved compared with the pure copper material of Comparative Example 1, reaching about 357 MPa, an increase of about 37%. This is mainly attributed to the chemical bridging effect of oxygen in the spherical PPy and the rich nitrogen element itself, which can change its chemical properties, increase the interface binding energy, and improve the interface bonding between the copper matrix and the spherical PPy, thereby increasing the interface bonding strength and significantly improving the strengthening effect of the reinforcement.
[0064] Example 2
[0065] A novel method for preparing a graphitized polypyrrole ball reinforced copper-based composite material, the specific steps are as follows:
[0066] (1) Preparation of graphitized polypyrrole nanospheres (G-PNSs) reinforcement
[0067] Weigh 3g of FeCl3·6H2O (99%) brown-yellow powder into a 500ml beaker, then add 100ml of deionized water for ultrasonic dispersion for 20min. After the ultrasonication, place it on a magnetic stirrer for stirring for later use. Subsequently, use a pipette to extract 420μL of pyrrole (98%) and slowly drip it into the FeCl3·6H2O solution, and stir it at room temperature for 24h. After that, functional PNSs powder is obtained by filtration and vacuum drying. After that, inert gas is introduced into a vacuum tube furnace for graphitization at 1000°C to obtain spherical particle G-PNSs powder with a particle size of 200nm, and the morphology is as follows. Figure 1 shown.
[0068] (2) Preparation of G-PNSs / Cu composite powder
[0069] 3 g of the graphitized polypyrrole ball (G-PNSs) powder obtained in step (1) and 150 g of hydrated copper acetate (CuAc·H2O) were weighed and ultrasonically dispersed in deionized water for 20 min respectively for later use. The G-PNSs dispersion solution was added to the CuAc·H2O solution and stirred in a water bath at 80°C for 60 min to obtain a G-PNSs / CuAc mixed solution. Subsequently, 90 g of sodium hydroxide (0.5 mol / L) and 70 g of glucose (0.8 mol / L) were weighed and dispersed into a solution and then added to the mixed solution in sequence. When the color of the solution changed from dark blue to brick red, stirring was stopped, and G-PNSs / Cu2O powder was obtained by filtration and vacuum drying. Finally, the above powder was reduced at 400°C for 300 min in a vacuum tube furnace with Ar / H2 as protective reducing gas at a heating rate of 10°C / min to obtain a G-PNSs / Cu composite powder.
[0070] (3) Preparation of G-PNSs / Cu composite closed-cell powder
[0071] The G-PNSs / Cu powder with holes obtained in step (2) was placed in a ball mill, and 1 / 3 of the volume of the ball mill was added with alcohol, and argon was used as the protective gas. After ball milling at a speed of 250 r / min for 180 min, the powder was vacuum dried to obtain a G-PNSs / Cu flaky composite powder. The flaky powder has a large specific surface area and can effectively improve the interface bonding between G-PNSs and the copper matrix. The morphology is as follows: Figure 2 shown.
[0072] (4) Preparation of G-PNSs / Cu composites
[0073] Weigh 300 g of the G-PNSs / Cu composite powder obtained in step (3) and evacuate the furnace body to vacuum (with Ar as protective gas) in a fast hot pressing sintering furnace (FHP), sinter at 700°C, keep warm for 15 minutes, turn off the vacuum, turn off the instrument, and take out the sample after the furnace cools to room temperature (about 20 minutes) to obtain a G-PNSs / Cu composite material.
[0074] Comparative Example 2
[0075] Weigh 300 g of Cu powder prepared by the MLM method, evacuate the furnace body into a vacuum (with Ar as the protective gas) in a fast hot pressing sintering furnace (FHP), and sinter at 700°C. After keeping warm for 15 minutes, turn off the vacuum and the instrument. After the furnace cools to room temperature (about 20 minutes), take out the sample to obtain a pure Cu block.
[0076] The conductivity and hardness of the composite materials prepared in Example 2 and Comparative Example 2 were tested. The results are as follows: Figure 7 As shown; for mechanical properties test, the results are as follows Figure 8 shown.
[0077] like Figure 7 As shown, the composite material prepared by molecular blending combined with rapid hot pressing sintering process has better performance than Example 1. The conductivity of the composite material of Example 2 is slightly higher than that of Comparative Example 2, which is mainly due to the further increase of the reinforcement content, which plays a role in improving the scattering of electrons in the transmission process. However, the excessive G-PNSs content (0.2wt%) causes large-area agglomeration of the reinforcement, resulting in debonding of the interface between G-PNSs and the matrix, which is also the reason why its hardness is reduced compared with Example 1.
[0078] like Figure 8 As shown, the tensile strength of the composite material of Example 2 is enhanced to a certain extent compared with the pure copper material of Comparative Example 2, but the effect is not significant. The enhancement mechanism is basically the same as that in Example 1.
[0079] Example 3
[0080] A novel method for preparing a graphitized polypyrrole ball reinforced copper-based composite material, the specific steps are as follows:
[0081] (1) Preparation of graphitized polypyrrole nanospheres (G-PNSs) reinforcement
[0082] Weigh 1.5g of FeCl3·6H2O (99%) brown-yellow powder into a 500ml beaker, then add 100ml of deionized water for ultrasonic dispersion for 20min. After ultrasonication, place it on a magnetic stirrer for stirring for later use. Subsequently, use a pipette to extract 420μL of pyrrole (98%) and slowly drip it into the FeCl3·6H2O solution, and stir it at room temperature for 24h. After that, functional PNSs powder is obtained by filtration and vacuum drying. After that, inert gas is introduced into a vacuum tube furnace for graphitization at 900°C to obtain G-PNSs powder with the morphology as shown in the figure. Figure 1 shown.
[0083] (2) Preparation of G-PNSs / Cu composite powder
[0084] 1.5 g and 70 g of the graphitized polypyrrole ball (G-PNSs) powder obtained in step (1) were weighed and ultrasonically dispersed in deionized water for 15 min respectively. The G-PNSs dispersion solution was added to the CuAc·H2O solution and stirred in a 70°C water bath for 45 min to obtain a G-PNSs / CuAc mixed solution. Subsequently, 45 g of sodium hydroxide (0.5 mol / L) and 45 g of glucose (0.8 mol / L) were weighed and dispersed into a solution and then added to the mixed solution in sequence. When the color of the solution changed from dark blue to brick red, stirring was stopped, and G-PNSs / Cu2O powder was obtained by filtration and vacuum drying. Finally, the above powder was reduced at 350°C for 250 min at a heating rate of 7°C / min in a vacuum tube furnace with Ar / H2 as protective reducing gas to obtain a G-PNSs / Cu composite powder.
[0085] (3) Preparation of G-PNSs / Cu composite closed-cell powder
[0086] The G-PNSs / Cu powder with holes obtained in step (2) was placed in a ball mill, and alcohol was added, and argon was used as a protective gas. After ball milling for 150 minutes, the powder was vacuum dried to obtain a G-PNSs / Cu flaky composite powder (flaky powder has a large specific surface area and can effectively improve the interface bonding between G-PNSs and the copper matrix), with a morphology as shown in FIG. Figure 2 shown.
[0087] (4) Preparation of G-PNSs / Cu composites
[0088] Weigh 160 g of the G-PNSs / Cu composite powder obtained in step (3), evacuate the furnace body to vacuum (with Ar as protective gas) in a fast hot pressing sintering furnace (FHP), sinter at 650°C, keep warm for 12 minutes, turn off the vacuum, turn off the instrument, and take out the sample after the furnace cools to room temperature (about 20 minutes) to obtain a G-PNSs / Cu composite material.
[0089] Comparative Example 3
[0090] Weigh 160 g of Cu powder prepared by the MLM method, evacuate the furnace body into a vacuum (with Ar as the protective gas) in a fast hot pressing sintering furnace (FHP), and sinter at 650°C. After keeping warm for 12 minutes, turn off the vacuum and the instrument. After the furnace cools to room temperature (about 20 minutes), take out the sample to obtain a pure Cu block.
[0091] The conductivity and hardness of the composite materials prepared in Example 3 and Comparative Example 3 were tested. The results are as follows: Figure 3 As shown; for mechanical properties test, the results are as follows Figure 4The performance of the composite material prepared in Example 3 is the best compared with that in Example 1 and Example 2; its reinforcement mechanism is that the reinforcement content reaches a moderate level, showing an excellent reinforcement effect, and other reinforcement mechanisms are basically the same as those in Example 1.
[0092] In summary, the present invention provides a method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material. The preparation method is simple, the experimental cycle is short and the practicability is strong. The obtained composite material can maintain good electrical conductivity while having high-strength performance. The chemical bridging reaction occurred by the molecular-level blending method, and the prepared G-PNSs exhibited obvious corrugated structure and strong roughness on its side wall, and further improved the interface bonding between G-PNSs and the copper matrix through the pinning effect, which can effectively solve the problems in the background technology. The prepared copper-based composite material exhibits excellent mechanical properties and electrical conductivity, and provides technical guidance for the development of high-performance copper-based composite materials, applied in the field of power electronic materials, especially used as cable materials, motor materials, lead frame materials and integrated circuit heat sink materials.
[0093] The embodiments described above are only preferred embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art through any modification, replacement, improvement, etc. without any innovation are within the protection scope of the present invention.
Claims
1. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material. Features: The method steps are as follows: (1) Preparation of graphitized polypyrrole nanospheres (G-PNSs) reinforcement Weigh 1g~3g FeCl 3 6H 2 O (99%) powder was placed in a beaker, and then 100 ml of deionized water was added for ultrasonic dispersion for 10 min to 20 min. After the ultrasonic dispersion was completed, the mixture was placed on a magnetic stirrer for stirring. Subsequently, 420 μL of pyrrole (98%) was drawn with a pipette and slowly dripped into the FeCl 3 6H 2 O solution and stirred at room temperature for 24 hours; then, functional PNSs powder was obtained by suction filtration and vacuum drying; then, inert gas was introduced into a vacuum tube furnace at 650°C to 1000°C for graphitization to obtain G-PNSs powder; (2) Preparation of G-PNSs / Cu composite powder Weigh appropriate amount of G-PNSs powder and CuAc·H 2 O were ultrasonically dispersed, and then the G-PNSs dispersion solution was added into CuAc·H 2 O solution was stirred in a water bath to obtain a G-PNSs / CuAc mixed solution, and then sodium hydroxide and glucose solution were added in sequence, and G-PNSs / Cu composite powder was obtained after stirring, filtering, drying and reducing operations; (3) Preparation of G-PNSs / Cu composite closed-cell powder The G-PNSs / Cu powder with holes obtained in step (2) is placed in a ball mill, alcohol is added, and argon is used as a protective gas. After ball milling for a certain period of time, the powder is vacuum dried to obtain a G-PNSs / Cu flaky composite powder; (4) Preparation of G-PNSs / Cu composites Weigh 30 g to 300 g of the G-PNSs / Cu composite powder obtained in step (3), evacuate the furnace body in a rapid hot pressing sintering furnace (FHP), sinter at 600° C. to 700° C., keep warm for 10 min to 15 min, turn off the vacuum, turn off the instrument, and take out the sample after the furnace cools to room temperature to obtain a G-PNSs / Cu composite block.
2. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 1, Features: The specific operation of step (2) is: Weigh 0.3 g to 3 g of graphitized polypyrrole spheres (G-PNSs) powder and 15 g to 150 g of hydrated copper acetate (CuAc·H 2 O) were ultrasonically dispersed in deionized water for 10 min to 20 min, and the G-PNSs dispersion solution was added to CuAc·H 2 O solution, stirred in a water bath environment at 60℃~80℃ for 30min~60min to obtain a G-PNSs / CuAc mixed solution, then weighed 9g~90g sodium hydroxide (0.5mol / L) and 7g~70g glucose (0.8mol / L) to disperse into a solution and then added to the above mixed solution in sequence, and the stirring was stopped when the color of the solution changed from dark blue to brick red, and the G-PNSs / CuAc was obtained by filtration and vacuum drying. 2 O powder, and finally, the above powder is reduced in a vacuum tube furnace at a certain temperature for a period of time to obtain G-PNSs / Cu composite powder.
3. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 1, Features: In step (1), the proportion of the G-PNSs powder is 0.1wt% to 0.2wt% (calculated based on the total amount); the particle size is 100nm to 200nm; and the morphology is spherical particles.
4. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 2, Features: In step (2), the CuAc·H 2 O was analytically pure (AR≥99%); NaOH was analytically pure (AR≥99%); glucose was analytically pure (AR≥99%).
5. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 2, Features: In step (2), the vacuum reduction heating rate is 5°C / min to 10°C / min, the holding temperature is 300°C to 400°C, the holding time is 200min to 300min, and the Ar / H 2 It is a protective reducing gas.
6. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 1 or 2, Features: In step (3), the amount of alcohol added is 1 / 4 to 1 / 3 of the volume of the ball mill; the ball-to-material ratio is 10:1 to 15:1; the ball milling time is 120 min to 180 min; and the ball milling speed is 200 r / min to 250 r / min.
7. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 1 or 2, Features: In step (4), the particle size of the G-PNSs / Cu composite powder is 20 μm to 50 μm; the morphology is spherical or flaky, or any irregular shape.
8. A method for preparing a novel graphitized polypyrrole ball reinforced copper-based composite material according to claim 1 or 2, Features: In step (4), the heating rate of the fast hot pressing sintering furnace (FHP) is 50°C / min to 100°C / min; the sintering temperature is 600°C to 700°C; and the holding time is 10min to 15min.
Citation Information
Cited By
Nanopore dispersion strengthened copper material and preparation method and application thereof
CN121380661A