Preparation method for precipitating secondary spheroidal graphite in nodular cast iron material
By melting and heat treatment of medium frequency induction furnaces in ductile iron materials, more, smaller and denser graphite balls are generated, which solves the problem of insufficient number of graphite balls in traditional materials, and significantly improves the aluminum liquid resistance of aluminum alloy die-casting molds The melting performance extends the service life of the mold.
Patent Information
- Application Number
- CN202411054829.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The small number of graphite balls in traditional ductile iron materials leads to poor resistance to liquid aluminum melting to aluminum alloy die-casting molds, making it difficult to generate more, smaller and denser graphite balls through traditional heat treatment methods.
A method of preparing ductile iron material, including melting, spheroidization and incubation treatment of medium frequency induction furnace, followed by high-temperature annealing and euthanizing temperature below to form pearlite decomposition and secondary spherical graphite tissue, increasing the number of graphite spheres and density.
It significantly improves the anti-melt effect of the material on aluminum melt, extends the service life of aluminum alloy die-casting molds, and blocks the melting of liquid aluminum by forming a denser array of graphite balls.
Smart Images

Figure CN118957415A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a preparation method for precipitation of secondary spheroidal graphite in ductile iron materials. Background Art
[0002] In recent years, lightweight manufacturing with aluminum alloy as the main consumable has developed rapidly and is in the ascendant. The application field is constantly expanding, the proportion of aluminum materials is continuously increasing, and die casting has become the main forming method. Aluminum profile die casting molds are mostly 4Cr5Mo2V1 series hot working die steels developed for the service environment of hot forging of steel parts. Although the mechanical properties meet the thermal strength requirements under die casting conditions, the mold is short-lived and high-consumption due to melt corrosion accelerated by aluminum heat reaction, which has become one of the main bottlenecks for improving the production efficiency of the aluminum industry. Therefore, how to obtain die casting mold materials with good resistance to aluminum liquid corrosion is of great engineering significance.
[0003] Reducing the aluminum / iron contact area can effectively inhibit the thermite reaction. By utilizing the physical property that graphite and aluminum do not wet below 800°C, graphite is generated in the prepared material structure to prevent aluminum liquid from melting the material matrix. Ductile iron material meets this characteristic, but the number of graphite balls in traditional ductile iron materials is limited, that is, the effect of blocking aluminum liquid is limited. Therefore, obtaining more graphite balls with smaller size and smaller spacing is of great significance to the aluminum alloy die-casting mold's resistance to aluminum liquid melting. Therefore, how to significantly increase the number of graphite balls in ductile iron structure has become a problem that needs to be solved urgently.
[0004] At present, traditional ductile iron cannot obtain more graphite nodules with smaller sizes and smaller spacing. According to materials theory, the amount of graphite obtained by liquid-solid phase change during casting is difficult to exceed this order of magnitude. At high temperatures, the carbon atoms in the liquid phase diffuse, precipitate and grow very quickly, and it is very easy to form relatively coarse eutectic graphite nodules. The solid-state phase change in the traditional heat treatment process cannot change the number of graphite nodules, and new graphite nuclei cannot be generated. It can only make the original eutectic graphite nodules grow. Therefore, there is an urgent need for a heat treatment method that can generate new graphite grains to obtain more graphite nodules with smaller sizes and smaller spacing. Summary of the invention
[0005] In view of the problems that the current aluminum alloy die-casting mold has poor anti-corrosion performance and the amount of graphite in traditional ductile iron materials is small, the present invention provides a preparation method for precipitation of secondary spheroidal graphite in ductile iron materials.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A preparation method for precipitation of secondary spheroidal graphite in ductile iron material is specifically implemented according to the following steps:
[0008] Step 1, weighing and mixing scrap steel, pig iron raw material, pretreatment agent, carburizer, inoculant, and spheroidizer;
[0009] Step 2, placing the scrap steel, pig iron raw material, pretreatment agent and carburizer weighed in step 1 in a medium frequency induction furnace to melt into molten iron;
[0010] Step 3, pouring molten iron into the ladle with spheroidizing agent, inoculant and covering agent on the bottom;
[0011] Step 4, after slagging, quickly pour the molten iron in step 3 into a prefabricated sand mold to form, and obtain ductile iron material after solidification;
[0012] Step 5, subjecting the ductile iron material obtained in step 4 to high temperature annealing treatment, so that the pearlite in the ductile iron material is decomposed and the carbon atoms are dissolved in the matrix;
[0013] Step 6, annealing the ductile iron material after high temperature annealing in step 5 below the eutectoid temperature so that secondary spheroidal graphite is precipitated in the structure.
[0014] Furthermore, the scrap steel in step 1 is Q235 steel, which is 25% to 90% by mass; the pig iron raw material is Q10 breaded iron, which is 10% to 75% by mass; the pretreatment agent is SiC, which is 0.3% to 0.9% by mass; and the recarburizer is high-purity graphite, which is 0.2% to 3.8% by mass.
[0015] Furthermore, in step 2, the melting temperature of the medium frequency induction furnace is 1530° C. to 1570° C., and the holding time is 2 to 5 minutes.
[0016] Further, the spheroidizer in step 3 is Si-Mg-Ca-RE-Al or NiMg30 alloy, and the Si-Mg-Ca-RE-Al spheroidizer includes the following components in mass fraction: Si: 44% to 48%, Mg: 5.8% to 6.5%, Ca: 2% to 3%, Re: 1% to 1.5%, Al: 0.4% to 0.6%, and the rest is Fe; the mass of the Si-Mg-Ca-RE-Al spheroidizer accounts for 1.0% to 1.2% of the total mass of the molten iron, and the residual Mg content in the ductile iron material is 0.03% to 0.05%; the NiMg30 alloy spheroidizer includes the following components in mass fraction: Ni: 70% to 75%, Mg: 25% to 30%, and the mass of the NiMg30 alloy spheroidizer accounts for 1.0% to 1.2% of the total mass of the molten iron;
[0017] The inoculant is Si-Ba-Ca, which includes the following components by mass fraction: Si: 66% to 69%, Ba: 3.9% to 4.0%, Ca: 1.3% to 1.7%, and the rest is Fe. The amount of the inoculant accounts for 0.6% to 0.8% of the total mass of the molten iron;
[0018] The covering agent is rust-free iron filings.
[0019] Furthermore, in step 4, the interval time for pouring the molten iron into the sand mold is no more than 20 seconds.
[0020] Furthermore, the ductile iron material of step 4 comprises the following components by mass percentage: C: 3.4% to 4.0%, Si: 1.0% to 2.6%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03% to 0.05%, Re: 0% to 0.04%, and the remainder is Fe and unavoidable impurities.
[0021] Furthermore, the specific method of high temperature annealing in step 5 is: heating the ductile iron material from room temperature to 900°C to 1100°C at a heating rate of 4°C / min to 7°C / min, then keeping it warm for 10h to 15h, and air cooling it to room temperature after it is taken out of the furnace.
[0022] Furthermore, the specific method of annealing below the eutectic temperature in step 6 is: heating the ductile iron material after high-temperature annealing from room temperature to 720°C to 750°C at a heating rate of 4°C / min to 7°C / min, then keeping it warm for 10h to 15h, and air-cooling it to room temperature after being taken out of the furnace.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention adopts a traditional sand casting method. The molding materials used in the method are cheap and easy to obtain, and the casting mold is simple to manufacture, so the production cost is low. The method prepares a ductile iron material with the structure of pearlite, ferrite and eutectic graphite spheres. The material is annealed at high temperature and annealed below the eutectoid temperature so that the pearlite is completely decomposed, and the supersaturated carbon atoms in the iron matrix are precipitated in the form of fine and dispersed secondary spherical graphite, and finally the eutectic graphite spheres and secondary spherical graphite with ferrite as the matrix and dispersed on the matrix are obtained. The graphite below 800°C does not infiltrate the aluminum liquid, that is, the graphite ball array can form a capillary barrier for the aluminum liquid to melt the matrix, and the graphite ball array isolates the bonding surface surface tension of the aluminum liquid from infiltrating the matrix. Therefore, secondary graphite nodules can be precipitated in the ductile iron structure of the present invention, so that the number of graphite nodules is increased, the size of the graphite nodules is reduced, and the distance between adjacent graphite nodules is shortened, thereby achieving a graphite distribution state of "increased number and reduced distance", which can significantly improve the material's anti-corrosion effect on molten aluminum, solves the problem of poor anti-aluminum liquid corrosion performance of the current aluminum alloy die-casting mold, and greatly improves the service life of the aluminum alloy die-casting mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The metallographic structure photos of a ductile iron material prepared in Example 2 of the present invention are as follows: Figure (a) shows the metallographic structure before corrosion, and Figure (b) shows the metallographic structure after corrosion;
[0026] Figure 2 This is a corrosion metallographic structure photograph of a ductile iron material prepared in Example 2 of the present invention after heat treatment;
[0027] Figure 3 It is the aluminum melting weight loss rate of a ductile iron material prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work also fall within the scope of protection of the present disclosure.
[0029] The present invention is described in detail with reference to the accompanying drawings and specific embodiments as follows:
[0030] The present invention is a preparation method for precipitation of secondary spheroidal graphite in ductile iron material, comprising the following steps:
[0031] Step 1, batching and melting of raw materials. According to the composition requirements of ductile iron materials and the composition of raw materials, the raw materials are calculated and prepared according to the percentages: Q235 scrap steel: 25% to 90%, Q10 breaded iron: 10% to 75%, SiC pretreatment agent: 0.3% to 0.9%, high-purity graphite recarburizer: 0.2% to 3.8%, silicon-barium-calcium inoculant: 0.6% to 0.8%, rare earth magnesium or nickel-magnesium spheroidizer: 1.0 to 1.2%.
[0032] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The smelting temperature of the medium frequency induction furnace is 1530° C. to 1570° C., and the insulation time is 2 to 5 minutes.
[0033] Step 3, pouring the molten iron obtained in step 2 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1480°C to 1520°C after the spheroidization and inoculation treatment.
[0034] The spheroidizing agent is Si-Mg-Ca-RE-Al or NiMg30 alloy, and the Si-Mg-Ca-RE-Al spheroidizing agent includes the following components according to mass fraction: Si: 44% to 48%, Mg: 5.8% to 6.5%, Ca: 2% to 3%, Re: 1% to 1.5%, Al: 0.4% to 0.6%, and the rest is Fe; the mass of the Si-Mg-Ca-RE-Al spheroidizing agent accounts for 1.0% to 1.2% of the total mass of the molten iron, and the residual Mg content in the ductile iron material is 0.03% to 0. .05%; NiMg30 alloy spheroidizer includes the following components according to mass fraction: Ni: 70%~75%, Mg: 25%~30%, the mass of NiMg30 alloy spheroidizer accounts for 1.0%~1.2% of the total mass of molten iron; the inoculant is Si-Ba-Ca, which includes the following components according to mass fraction: Si: 66%~69%, Ba: 3.9%~4.0%, Ca: 1.3%~1.7%, and the rest is Fe. The amount of inoculant accounts for 0.6%~0.8% of the total mass of molten iron; the covering agent is rust-free iron filings.
[0035] Step 4, quickly pouring the melt after spheroidization and inoculation in step 3 into a sand mold to form, and obtaining a ductile iron material after solidification, the interval time of pouring the molten iron into the sand mold is not more than 20s, and the composition of the ductile iron material is C: 3.4% ~ 4.0%, Si: 1.0% ~ 2.6%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03% ~ 0.05%, Re: 0% ~ 0.04%, and the balance is Fe and unavoidable impurities.
[0036] Step 5, high temperature annealing treatment is performed on the ductile iron material, so that the pearlite in the ductile iron material is decomposed and the carbon atoms are dissolved in the iron matrix. The high temperature annealing treatment is specifically as follows: the ductile iron material is heated from room temperature to 900℃~1100℃ at a heating rate of 4℃ / min~7℃ / min, and then kept warm for 10h~15h, and then quenched or air-cooled to room temperature to complete the high temperature annealing treatment. The pearlite in the ductile iron material structure is decomposed by high temperature annealing treatment, and the carbon atoms are dissolved in the iron matrix.
[0037] Step 6, anneal the casting after high temperature annealing below the eutectoid temperature to precipitate secondary spheroidal graphite in the structure. The annealing treatment below the eutectoid temperature is specifically as follows: the ductile iron material after high temperature annealing is heated from room temperature to 720°C to 750°C at a heating rate of 4°C / min to 7°C / min, then kept warm for 10h to 15h, removed from the furnace and air-cooled to room temperature, completing the annealing treatment below the eutectoid temperature. After annealing below the eutectoid temperature, fine secondary spheroidal graphite is precipitated evenly distributed in the structure.
[0038] Example 1
[0039] Step 1, ingredients and melting of raw materials. Calculate and prepare each raw material according to the percentage: Q235 scrap steel: 90%, Q10 bread iron: 10%, SiC pretreatment agent: 0.3%, high purity graphite recarburizer: 3.8%, silicon barium calcium inoculant: 0.8%, nickel magnesium spheroidizer: 1.2%;
[0040] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The melting temperature of the medium frequency induction furnace is 1530° C. and the insulation time is 3 minutes.
[0041] Step 3, pouring the 1530°C molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1480°C after spheroidization and inoculation treatment.
[0042] Step 4, quickly pouring the melt after spheroidization and inoculation in step 2 into a sand mold to form, and obtaining a ductile iron material after solidification, wherein the composition of the ductile iron material is C: 4.0%, Si: 1.0%, Mn: 0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.05%, and the remainder is Fe.
[0043] Step 5, heating the ductile iron material from room temperature to 1100°C at a heating rate of 7°C / min, then keeping the temperature for 15 hours, taking it out of the furnace and air-cooling it to room temperature to complete the high temperature annealing treatment.
[0044] Step 6, heating the ductile iron material after high temperature annealing from room temperature to 720°C at a heating rate of 6°C / min, then keeping the temperature for 15 hours, taking it out of the furnace and air cooling it to room temperature, thus completing the annealing treatment below the eutectoid temperature.
[0045] Example 2
[0046] Step 1, ingredients and melting of raw materials. Calculate and prepare each raw material according to the percentage: Q235 scrap steel: 75%, Q10 bread iron: 25%, SiC pretreatment agent: 0.73%, high purity graphite recarburizer: 2.9%, silicon barium calcium inoculant: 0.8%, nickel magnesium spheroidizer: 1.2%.
[0047] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The melting temperature of the medium frequency induction furnace is 1540° C. and the insulation time is 3 minutes.
[0048] Step 3, pouring the 1540°C molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1490°C after spheroidization and inoculation treatment.
[0049] Step 4, quickly pouring the melt after spheroidization and inoculation in step 2 into a sand mold to form, and obtaining a ductile iron material after solidification, wherein the composition of the ductile iron material is C: 3.9%, Si: 1.4%, Mn: 0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.05%, and the remainder is Fe.
[0050] Step 5, heating the ductile iron material from room temperature to 1050°C at a heating rate of 6°C / min, then keeping the temperature for 12 hours, taking it out of the furnace and air-cooling it to room temperature to complete the high temperature annealing treatment.
[0051] Step 6, heating the ductile iron material after high temperature annealing from room temperature to 725°C at a heating rate of 4°C / min, then keeping the temperature for 15 hours, taking it out of the furnace and air cooling it to room temperature, thus completing the annealing treatment below the eutectoid temperature.
[0052] Figure 1 The metallographic structure photos of a ductile iron material prepared in Example 2 are as follows: Figure (a) is the metallographic structure before corrosion, and Figure (b) is the metallographic structure after corrosion; Figure 2 This is a corrosion metallographic structure photograph of a ductile iron material prepared in Example 2 after heat treatment.
[0053] Depend on Figure 1 and Figure 2 It can be seen that the number of graphite balls increases, the size decreases, and the distance between adjacent graphite balls decreases. The graphite ball array forms a capillary barrier to the aluminum liquid melting the matrix, and the graphite ball array isolates the surface tension of the bonding surface from the aluminum liquid infiltration of the matrix, which solves the current problem of poor aluminum liquid corrosion resistance of aluminum alloy die-casting molds.
[0054] Figure 3 is the aluminum melting weight loss rate of a ductile iron material prepared in Example 2, Figure 3 The results show that the aluminum melting weight loss rate of the ductile iron material prepared with secondary spheroidal graphite precipitation in this embodiment is reduced by about half compared with the traditional H13 steel aluminum die-casting mold. Therefore, the present invention can greatly improve the service life of the aluminum alloy die-casting mold.
[0055] Example 3
[0056] Step 1, ingredients and melting of raw materials. Calculate and prepare each raw material according to the percentage: Q235 scrap steel: 60%, Q10 bread iron: 40%, SiC pretreatment agent: 0.43%, high purity graphite recarburizer: 2.1%, silicon barium calcium inoculant: 0.8%, rare earth magnesium spheroidizer: 1.1%.
[0057] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The melting temperature of the medium frequency induction furnace is 1550° C. and the insulation time is 3 minutes.
[0058] Step 3, pouring the 1550°C molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1500°C after spheroidization and inoculation treatment.
[0059] Step 4, quickly pouring the melt after spheroidization and inoculation in step 2 into a sand mold to form, and obtaining a ductile iron material after solidification, wherein the composition of the ductile iron material is C: 3.7%, Si: 1.8%, Mn: 0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.04%, Re: 0.03%, and the remainder is Fe.
[0060] Step 5, heating the ductile iron material from room temperature to 1000°C at a heating rate of 6°C / min, then keeping the temperature for 12 hours, taking it out of the furnace and air-cooling it to room temperature to complete the high temperature annealing treatment.
[0061] Step 6, heating the ductile iron material after high temperature annealing from room temperature to 735°C at a heating rate of 4°C / min, then keeping the temperature for 15 hours, taking it out of the furnace and air cooling it to room temperature, thus completing the annealing treatment below the eutectoid temperature.
[0062] Example 4
[0063] Step 1, ingredients and melting of raw materials. Calculate and prepare each raw material according to the percentage: Q235 scrap steel: 40%, Q10 bread iron: 60%, SiC pretreatment agent: 0.78%, high purity graphite recarburizer: 1.0%, silicon barium calcium inoculant: 0.8%, rare earth magnesium spheroidizer: 1.1%.
[0064] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The melting temperature of the medium frequency induction furnace is 1560° C. and the insulation time is 3 minutes.
[0065] Step 3, pouring the 1560°C molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1510°C after spheroidization and inoculation treatment.
[0066] Step 4, quickly pouring the melt after spheroidization and inoculation in step 2 into a sand mold to form, and obtaining a ductile iron material after solidification, wherein the composition of the ductile iron material is C: 3.6%, Si: 2.2%, Mn: 0.3%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03%, Re: 0.03%, and the balance is Fe.
[0067] Step 5, heating the ductile iron material from room temperature to 950°C at a heating rate of 5°C / min, then keeping the temperature for 10 hours, taking it out of the furnace and air-cooling it to room temperature to complete the high temperature annealing treatment.
[0068] Step 6, heating the ductile iron material after high temperature annealing from room temperature to 740°C at a heating rate of 5°C / min, then keeping the temperature for 15 hours, taking it out of the furnace and air cooling it to room temperature, thus completing the annealing treatment below the eutectoid temperature.
[0069] Example 5
[0070] Step 1, ingredients and melting of raw materials. Calculate and prepare each raw material according to the percentage: Q235 scrap steel: 25%, Q10 bread iron: 75%, SiC pretreatment agent: 1.26%, high purity graphite recarburizer: 0.18%, silicon barium calcium inoculant: 0.8%, rare earth magnesium spheroidizer: 1.0%
[0071] Step 2: Put the weighed scrap steel, raw iron and carburizer raw materials into a medium frequency induction furnace and heat them to melt into molten iron. The melting temperature of the medium frequency induction furnace is 1570° C. and the insulation time is 3 minutes.
[0072] Step 3, pouring the 1570°C molten iron obtained in step 1 into a ladle with a spheroidizing agent, an inoculant and a covering agent pre-laid on the bottom for spheroidization and inoculation treatment, and controlling the temperature of the molten iron to be 1520°C after spheroidization and inoculation treatment.
[0073] Step 4, quickly pouring the melt after spheroidization and inoculation in step 2 into a sand mold to form, and obtaining a ductile iron material after solidification, wherein the composition of the ductile iron material is C: 3.4%, Si: 2.6%, Mn: 0.4%, S: ≤0.02%, P: ≤0.1%, Mg: 0.04%, Re: 0.02%, and the balance is Fe.
[0074] Step 5, heating the ductile iron material from room temperature to 900°C at a heating rate of 4°C / min, then keeping the temperature for 10 hours, taking it out of the furnace and air-cooling it to room temperature to complete the high temperature annealing treatment.
[0075] Step 6, heating the ductile iron material after high temperature annealing from room temperature to 750°C at a heating rate of 4°C / min, then keeping the temperature for 10 hours, taking it out of the furnace and air cooling it to room temperature, thus completing the annealing treatment below the eutectoid temperature.
[0076] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be considered to fall within the protection scope of the present invention.
Claims
1. A method for preparing secondary spheroidal graphite precipitation in ductile iron material, characterized in that: Follow the steps below to implement it: Step 1, weighing and mixing scrap steel, pig iron raw material, pretreatment agent, carburizer, inoculant, and spheroidizer; Step 2, placing the scrap steel, pig iron raw material, pretreatment agent and carburizer weighed in step 1 in a medium frequency induction furnace to melt into molten iron; Step 3, pouring molten iron into the ladle with spheroidizing agent, inoculant and covering agent on the bottom; Step 4, after slagging, quickly pour the molten iron in step 3 into a prefabricated sand mold to form, and obtain ductile iron material after solidification; Step 5, subjecting the ductile iron material obtained in step 4 to high temperature annealing treatment, so that the pearlite in the ductile iron material is decomposed and the carbon atoms are dissolved in the matrix; Step 6, annealing the ductile iron material after high temperature annealing in step 5 below the eutectoid temperature so that secondary spheroidal graphite is precipitated in the structure.
2. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: The scrap steel in step 1 is Q235 steel, which accounts for 25% to 90% by mass; the pig iron raw material is Q10 breaded iron, which accounts for 10% to 75% by mass; the pretreatment agent is SiC, which accounts for 0.3% to 0.9% by mass; and the recarburizer is high-purity graphite, which accounts for 0.2% to 3.8% by mass.
3. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: Step 2: The melting temperature of the medium frequency induction furnace is 1530°C to 1570°C, and the holding time is 2 to 5 minutes.
4. The method for preparing secondary spheroidal graphite in ductile iron material according to claim 1, characterized in that: The spheroidizer in step 3 is Si-Mg-Ca-RE-Al or NiMg30 alloy, and the Si-Mg-Ca-RE-Al spheroidizer includes the following components by mass fraction: Si: 44% to 48%, Mg: 5.8% to 6.5%, Ca: 2% to 3%, Re: 1% to 1.5%, Al: 0.4% to 0.6%, and the rest is Fe; the mass of the Si-Mg-Ca-RE-Al spheroidizer accounts for 1.0% to 1.2% of the total mass of the molten iron, and the residual Mg content in the ductile iron material is 0.03% to 0.05%; the NiMg30 alloy spheroidizer includes the following components by mass fraction: Ni: 70% to 75%, Mg: 25% to 30%, and the mass of the NiMg30 alloy spheroidizer accounts for 1.0% to 1.2% of the total mass of the molten iron; The inoculant is Si-Ba-Ca, which includes the following components by mass fraction: Si: 66% to 69%, Ba: 3.9% to 4.0%, Ca: 1.3% to 1.7%, and the rest is Fe. The amount of the inoculant accounts for 0.6% to 0.8% of the total mass of the molten iron; The covering agent is rust-free iron filings.
5. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: In step 4, the interval time for pouring molten iron into the sand mold is no more than 20s.
6. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: The ductile iron material of step 4 comprises the following components by mass percentage: C: 3.4% to 4.0%, Si: 1.0% to 2.6%, Mn: ≤0.6%, S: ≤0.02%, P: ≤0.1%, Mg: 0.03% to 0.05%, Re: 0% to 0.04%, and the remainder is Fe and unavoidable impurities.
7. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: The specific method of high temperature annealing in step 5 is: the ductile iron material is heated from room temperature to 900°C to 1100°C at a heating rate of 4°C / min to 7°C / min, then kept warm for 10h to 15h, and air-cooled to room temperature after being taken out of the furnace.
8. The method for preparing secondary spheroidal graphite in a ductile iron material according to claim 1, characterized in that: The specific method of annealing below the eutectoid temperature in step 6 is as follows: the ductile iron material after high temperature annealing is heated from room temperature to 720°C to 750°C at a heating rate of 4°C / min to 7°C / min, then kept warm for 10h to 15h, and then air-cooled to room temperature after being taken out of the furnace.
Citation Information
Patent Citations
Nodular iron casting for heavy axle main speed reducer shell and preparation process of nodular iron casting
CN109576567A
Nodular cast iron and preparation method thereof
CN117604371A
Nodular cast iron material, preparation method and nodular cast iron manufactured part
CN118147517A
High toughness spheroidal graphite cast iron and method for producing the same
US3891432A
Cited By
QT450-10LT high-strength and high-toughness low-temperature nodular cast iron and preparation method thereof
CN119614991A
Nodular cast iron and preparation method and application thereof
CN120026240A