Low-cost easy-to-form hot-rolled high-weathering-resistance steel and preparation method thereof

By optimizing the alloy element combination and process flow of weathering steel, uniform ferrite and pearlite structure are formed, and the problems of high cost and poor molding performance of existing weathering steels are solved, achieving low-cost, easy-to-form and high weathering matching , meets the requirements of high strength and good moldability.

CN118957446APending Publication Date: 2024-11-15HANDAN IRON & STEEL GROUP CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410972994.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

While pursuing high weather resistance and high strength, existing weather-resistant steels have high costs and poor molding performance. Especially the application of hot-rolled thin strip steels is limited, making it difficult to achieve a good match between low cost, easy molding and high weather resistance.

Method used

By optimizing the alloy element combination relationship, using the special ratios of C, Si, Mn, P, Cu, Cr, and Ni, a low-cost, easy-to-form, hot-rolled, high-weather-resistant steel is designed with chemical compositions of C: 0.08~0.10, Si: 0.30 ~0.40, Mn: 0.40~0.50, P: 0.07~0.13, S≤0.006, Al: 0.020~0.030, Nb: 0.006~0.015, Ti: 0.008~0.018, Cu: 0.25~0.40, Cr: 0.35~0.75, Ni ≤0.05, combined with converter smelting, LF refining, continuous casting, controlled rolling and cooling and coiling processes, the solid solution and cooling process of alloy elements are controlled to form uniform ferrite and pearlite structure.

Benefits of technology

Achieve good matching with low cost, easy molding and high weather resistance. The yield strength of the steel plate is 421~465MPa, tensile strength is 537~587MPa, elongation rate is 30~33.5%, and the 72h cycle infiltration corrosion rate is ≤1.50 g/(m2·h) , reduces alloy costs and achieves stable batch industrial production on conventional production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957446A_ABST
    Figure CN118957446A_ABST
Patent Text Reader

Abstract

The invention discloses low-cost easy-to-form hot-rolled high-weathering-resistant steel and a production method thereof. The weathering-resistant steel comprises the following chemical components: 0.08 to 0.10 percent of C, 0.30 to 0.40 percent of Si, 0.40 to 0.50 percent of Mn, 0.07 to 0.13 percent of P, less than or equal to 0.006 percent of S, 0.020 to 0.030 percent of Als, 0.006 to 0.015 percent of Nb, 0.008 to 0.018 percent of Ti, 0.25 to 0.40 percent of Cu, 0.35 to 0.75 percent of Cr, less than or equal to 0.05 percent of Ni and the balance of Fe and inevitable impurities. In addition, the chemical components meet the condition that T is larger than or equal to 810 and smaller than or equal to 820, and T = 810 + 275 [P]-21 [Cu]-25 [Cr]-36 [Ni]. The production method comprises the procedures of converter smelting, LF refining, continuous casting, casting blank heating, controlled rolling and controlled cooling and coiling. The weathering steel provided by the invention is low in cost and excellent in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of weathering steel production, and specifically relates to a low-cost, easy-to-form hot-rolled high-weathering steel and a preparation method thereof. Technical Background

[0002] Weathering steel is widely used in steel structure construction fields such as building bridges, railway vehicles, power towers, container plates, etc. due to its excellent weather resistance, cost controllability and easy production and processing. In order to obtain high weather resistance and high strength, a large amount of weathering elements Cu, Cr, Ni, Nb, and Ti are usually added, especially the expensive Ni and Nb elements, which will inevitably increase the cost. P is cheap and can significantly improve the weather resistance of steel, but it is not good for low temperature toughness and cold forming; at the same time, considering that weathering structural steel needs to undergo processing such as bending, shearing and stretching of the mold to make the thin plate or strip plastically deformed to obtain the required shape and size; in order to ensure the processability, higher requirements are put forward on the forming performance of weathering steel.

[0003] The invention patent with authorization announcement number CN103695801B discloses a high-toughness, high-weathering steel and its manufacturing method, which uses Cu, Cr, Ni, and P microalloying composition design to ensure high weathering resistance, and Nb microalloying to improve low-temperature toughness, to obtain a steel plate with a yield strength of 355MPa and an elongation of ≥22%, which cannot meet the requirements of strength and easy forming. At the same time, the finished steel plate has a thickness of 12 to 35mm, which is common in medium and thick plate products, and is not applicable to hot-rolled thin strip steel.

[0004] The invention patent with authorization announcement number CN113201685B provides an economical low yield ratio hot-rolled weathering steel plate and its manufacturing method, and the invention patent with publication number CN113373378A provides an economical high weathering resistant medium and thick Q355GNH steel plate and its production method. Through the composition design of Cu, Cr and Ni micro-alloying, it has high weather resistance. However, due to the absence of Nb and Ti elements, the yield strength of the steel plate cannot reach 415MPa relying solely on the solid solution strengthening of Cu, Cr and Ni elements.

[0005] The invention patent with authorization announcement number CN114657467B provides a method for producing weathering steel plates with a yield strength of 415MPa, which controls the higher Ni and Nb contents, resulting in a significant increase in alloy costs.

[0006] The 400MPa grade high chromium weathering steel and its preparation method provided by the invention patent with publication number CN111850411A, and the 480MPa grade high silicon high chromium weathering steel and its preparation method provided by the invention patent with publication number CN111690878A, are both designed with a high Cr component of 1.2 to 2.0wt%, have high weather resistance, but increase the alloy cost. At the same time, the elongation of the steel plate is low and does not have good formability.

[0007] The invention patent with authorization announcement number CN110284053B provides a high-P, high-strength, high-toughness, high-weather resistance hot-rolled steel and its manufacturing method, which adopts a high-P content of 0.10-0.15wt% and a composition design without Ni and Cr. Although the alloy cost is reduced, it does not have good weather resistance.

[0008] The invention patent with authorization announcement number CN106367681B, "A process for preparing low-cost ultra-low-carbon steel plates for railway carriages", controls Cu, Cr, and Ni at a relatively low level, significantly reducing costs; by regulating the hot rolling process, an oxide scale Fe3O4 with anti-corrosion properties is obtained on the surface of the steel plate, but compared with the dense rust layer α-FeOOH formed on the surface of weathering steel, it does not have good weather resistance.

[0009] Therefore, how to optimize the composition and process of the current 415MPa grade hot-rolled weathering steel strip to obtain uniform ferrite and pearlite structure, and achieve a good match of low cost, easy forming and high weather resistance while ensuring that the strength meets the requirements, is a key technical issue that urgently needs to be broken through in the current field of weathering structural steel material design and manufacturing technology. Summary of the invention

[0010] The present invention aims to provide a low-cost, easy-to-form hot-rolled high-weathering steel, whose room temperature structure is composed of ferrite and pearlite, with a ferrite content of 80-90%; a yield strength of 421-465MPa, a tensile strength of 537-587MPa, a yield strength ratio of 0.77-0.80, an elongation of 30-33.5%, and a 72h periodic immersion corrosion rate of ≤1.50 g / (m 2 ·h), the cost is greatly reduced compared with conventional weathering steel, achieving a good match of low cost, easy forming and high weathering resistance; the present invention also provides a preparation method of low-cost, easy-forming hot-rolled high weathering steel.

[0011] To achieve the above object, the present invention proposes the following technical solutions: A low-cost, easy-to-form hot-rolled high-weathering steel, the chemical composition of which is calculated by weight percentage as follows: C: 0.08-0.10, Si: 0.30-0.40, Mn: 0.40-0.50, P: 0.07-0.13, S≤0.006, Als: 0.020-0.030, Nb: 0.006-0.015, Ti: 0.008-0.018, Cu: 0.25-0.40, Cr: 0.35-0.75, Ni≤0.05, the balance is Fe and unavoidable impurities; in addition, the chemical composition must also meet 810≤T≤820, wherein T=810+275[P]-21[Cu]-25[Cr]-36[Ni].

[0012] The design principle of the alloy element combination relationship T of the present invention is as follows: The alloy element combination relationship T of the weathering steel described in the present invention is based on an empirical formula for the starting temperature of the transformation from austenite to ferrite in low carbon steel. It takes into account the particularity of the key alloy elements P, Cu, Cr, and Ni in the actual production of the steel of the present invention, and is obtained by solidifying the basic stable and controllable elements C, Si, Mn, Nb, and Ti in steelmaking production.

[0013] For the weathering steel described in the present invention, C, Si, and Mn, as the most basic elements in low carbon steel, provide a significant solid solution strengthening effect; Nb and Ti, as elements commonly used in low carbon microalloy steel, their precipitated phases can not only pin the austenite grain boundaries and refine the austenite grains during the recrystallization process of rough rolling, but also play a precipitation strengthening role during the deformation process of fine rolling. These two types of elements have been used as basic elements in the composition design of weathering steel, and a large number of experimental studies have been conducted. At the same time, their stable and controllable characteristics are also widely applicable in industrial production.

[0014] The key alloying elements P, Cu, Cr and Ni in the steel of the present invention have obvious particularity, which is mainly reflected in the following three aspects: First, P, Cu, Cr, and Ni are all weather-resistant elements. The combined use of P and Cu can improve the atmospheric corrosion resistance of low-alloy steel. Cr can promote the formation of a dense inner rust layer, and Ni can improve the density of corrosion products. Therefore, the content of P, Cu, Cr, and Ni has a significant effect on the growth of the rust layer of weathering steel, thereby affecting the safety and service life of structural parts.

[0015] Secondly, P is a ferrite strengthening element, while Cu, Cr and Ni can improve hardenability. Both of them will improve the strength and hardness of weathering steel and are not conducive to its formability. This requires limiting the upper limit of the content of P, Cu, Cr and Ni. At the same time, different cooling rate tests need to be carried out to establish the corresponding relationship between composition and cooling rate.

[0016] Third, during the solid-state transformation of steel, P can significantly increase the starting transformation temperature of γ→α, while Cu, Cr, and Ni play the opposite role. Therefore, the content ratio of P, Cu, Cr, and Ni is very important for the structural transformation of steel, which in turn affects the mechanical properties of structural parts. Therefore, in addition to limiting the range of each element, it is also necessary to control its combined content.

[0017] The low-cost, easy-to-form hot-rolled high-weathering steel finished product of the present invention has a thickness of 2 to 8 mm.

[0018] The low-cost, easy-to-form hot-rolled high-weathering steel of the present invention has a room temperature structure composed of ferrite and pearlite, wherein the ferrite content is 80-90%; the yield strength is 421-465MPa, the tensile strength is 537-587MPa, the yield strength ratio is 0.77-0.80, the elongation is 30-33.5%, and the 72h periodic immersion corrosion rate is ≤1.50 g / (m 2 h).

[0019] The method for preparing the low-cost, easy-to-form hot-rolled high-weathering steel of the present invention comprises converter smelting, LF refining, continuous casting, billet heating, controlled rolling and controlled cooling, and coiling steps.

[0020] Preferably, in the method for preparing the low-cost, easy-to-form hot-rolled high-weathering steel of the present invention, in order to ensure that the alloy elements can be completely dissolved in the steel, the heating time of the casting is 150 to 200 minutes and the furnace temperature is 1180 to 1210°C.

[0021] Preferably, in the method for preparing low-cost, easy-to-form hot-rolled high-weathering steel of the present invention, the controlled rolling and controlled cooling process has a rough rolling outlet temperature of 1020-1050°C, a finishing rolling inlet temperature of 1000-1020°C, and a final rolling temperature of 880-910°C; in order to regulate the structural transformation during the cooling process, the average cooling rate of the post-rolling laminar cooling needs to be CR Controlled at 20-25℃ / s, and the above alloy element combination T and the average cooling rate of laminar cooling should be CR The secondary combination Ar3=T-6.2 CR Controlled between 660 and 690.

[0022] Preferably, in the method for preparing the low-cost, easy-to-form hot-rolled high-weathering steel of the present invention, in the coiling process, the coiling temperature is 500-530°C.

[0023] The design ideas of the weathering steel production process of the present invention are as follows: The "low temperature and short time" austenitizing process is adopted. Due to the low content of Nb and Ti, the required solid solution temperature is low. Therefore, the lower furnace temperature can not only ensure the solid solution of alloy elements, but also avoid the growth of austenite grains, which not only improves the efficiency of the production line but also reduces the process cost.

[0024] The controlled rolling and cooling process of "high temperature final rolling" + "rapid cooling after rolling" + "medium temperature coiling" is adopted. On the one hand, the growth of ferrite grains is avoided to prevent the problem of insufficient strength; on the other hand, the formation range of hardened structure is avoided, which effectively reduces the yield ratio and improves the elongation.

[0025] In the production practice of the steel of the present invention, in addition to the need to reasonably control the key process parameters of each process, the relationship between the laminar cooling rate and the microstructure and performance after cooling transformation is also considered, and then the secondary combination relationship between the alloy element combination and the average laminar cooling rate is obtained.

[0026] The usual empirical formula only includes the influence of alloying elements on the phase transition temperature, and does not consider the cooling rate factor, so the transformation temperature obtained is an ideal case. Since the structural transformation requires supercooling, the role of cooling rate cannot be ignored. The present invention has conducted a large number of practical studies and obtained the optimal average cooling rate range suitable for the steel of the present invention. On the basis of the empirical formula, the influence of the average cooling rate is supplemented, and the parameters in the empirical formula are optimized. At the same time, through laboratory research, it is clarified that the steel of the present invention obtains the phase transformation supercooling of uniform ferrite and pearlite, thereby limiting the transformation start temperature to 660-690°C, creating kinetic conditions for the ferrite structural transformation and ensuring that the transformation temperature falls within the range of ferrite and pearlite.

[0027] There is a certain correspondence between the coiling temperature and the laminar cooling rate. When the coiling temperature target value is set, the cooling secondary model automatically adjusts the water volume to meet the preset value of the coiling temperature. After a large number of field tests and studies, when the coiling temperature is controlled in the range of 500-530°C, the supercooled austenite phase transformation occurs in the cooling stage, thereby obtaining the ideal ferrite and pearlite structure. Since the diffusion type transformation takes time, if the coiling temperature is too high, the water volume of the secondary model is reduced, the cooling rate is reduced, and the supercooled austenite phase transformation not only occurs in the cooling stage, but also continues to transform after coiling. At this time, the ferrite and pearlite obtained are large in size, which is not conducive to strength control; if the coiling temperature is too low, the water volume of the secondary model increases, the cooling rate increases, and the supercooled austenite phase transformation occurs in the cooling stage. Due to its large degree of supercooling, the phase transformation product is prone to granular bainite, Widmanstatten structure and other hardened structures, which reduces the elongation and is not conducive to formability.

[0028] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) Low cost and easy process control. The content of expensive metal elements Ni and Nb is reduced, and the composition design idea of ​​replacing Ni with P and Nb with Ti is adopted. On the one hand, the weather resistance index I ≥ 7.0 is maintained, and on the other hand, the yield strength is ensured to meet the 415MPa level. At the same time, the steelmaking and rolling processes are easy to control, and conventional hot rolling production lines can achieve low-cost batch industrialized stable production.

[0029] (2) Uniform organization and excellent performance. The room temperature organization is composed of ferrite and pearlite, with a ferrite content of 80-90%, a yield strength of 421-465MPa, a tensile strength of 537-587MPa, a yield strength ratio of 0.77-0.80, an elongation of 30-33.5%, and a 72h cycle immersion corrosion rate of ≤1.50 g / (m 2 h); not only does the strength meet the requirements, but it also achieves a good match of low cost, easy molding and high weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the metallographic structure of the weathering steel in Example 1.

[0031] Figure 2 This is the metallographic structure of the weathering steel of comparative example 2.

[0032] Figure 3 This is the metallographic structure of the weathering steel of comparative example 3. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific examples and comparative examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Unless otherwise specified, the examples are all based on conventional experimental conditions. In addition, for those skilled in the art, without departing from the essence and scope of the present invention, various modifications or improvements to the material composition and dosage in these embodiments all belong to the scope of protection claimed in the present invention.

[0034] The chemical composition and content of the weathering steel of each embodiment and comparative example are shown in Table 1. In Table 1, T=810+275[P]-21[Cu]-25[Cr]-36[Ni].

[0035] Table 1 Chemical composition and content of weathering steel in various embodiments and comparative examples (%)

[0036] The weathering steels in each embodiment and comparative example are produced by three steps of converter smelting, LF refining and continuous casting, and the process parameters meet the following requirements: converter terminal temperature of 1610-1660°C, steel tapping time of 5-8 min, refining outlet temperature of 1560-1590°C, refining time of 30-45 min, continuous casting tundish temperature of 1525-1545°C, and liquid level fluctuation of no more than ±4 mm.

[0037] Considering the temperature drop of molten steel during transportation, the temperature and time of converter, refining and continuous casting are controlled to ensure the stability of steelmaking process, improve the fluidity of molten steel, reduce inclusions and impurities in molten steel, and obtain uniform molten steel composition. In order to give full play to the lubrication and heat transfer balance of crystallizer protection slag, reduce the risk of slag rolling, and ensure the quality of ingot, the liquid level fluctuation is controlled within ±4mm. The specific control process parameters of steelmaking are shown in Table 2.

[0038] Table 2 Steelmaking process parameters of various embodiments and comparative examples

[0039] After forming the continuous casting billet, the hot rolled coil is produced through three steps: billet heating, controlled rolling and controlled cooling, and coiling. The process parameters meet the following requirements: billet heating time is 150-200min, and the furnace temperature is 1180-1210℃; considering the recrystallization process and rolling stability, the rough rolling outlet temperature is 1020-1050℃, the finishing rolling inlet temperature is 1000-1020℃, and the final rolling temperature is 880-910℃; in order to control the organizational transformation of the cooling process, the post-rolling rapid cooling mode is adopted, the cooling rate is 20-25℃ / s, the coiling temperature is 500-530℃, and the finished product thickness is 2-8mm. The specific control process parameters of hot rolling are shown in Table 3.

[0040] Table 3 Hot rolling process parameters of various embodiments and comparative examples

[0041] Note: Ar3=T-6.2 in Table 3 CR .

[0042] The properties of the weathering steels of the embodiments and comparative examples are shown in Table 4.

[0043] Table 4 Weathering steel properties of various embodiments and comparative examples

[0044] As shown in Table 4, by using the composition and preparation process of the present invention, the yield strength of the steel strip is 421-465 MPa, the tensile strength is 537-587 MPa, the yield strength ratio is 0.77-0.80, the elongation is 30-33.5%, and the 72h periodic immersion corrosion rate is ≤1.50 g / (m 2 h).

[0045] Example 1 The metallographic structure of the steel strip is as follows Figure 1 As shown in the figure, it can be seen that its microstructure is uniform, consisting of ferrite and pearlite, of which the ferrite content is 86%. The microstructures of the other steel strips are also composed of ferrite and pearlite, with the ferrite content ranging from 80% to 90%.

[0046] Comparative Example 1 uses Cu, Cr, and Ni to improve corrosion resistance, and has excellent performance, but the cost is much higher than the weathering steel of the present invention; Comparative Example 2 uses the weathering steel composition provided by the present invention, and adopts sparse cooling and high-temperature coiling process. The microstructure of the weathering steel is coarse ferrite and pearlite, such as Figure 2 As shown, the ferrite content is 95%, the strength is low, and it fails to meet the strength requirements of the weathering steel of the present invention; the composition of comparative example 3 adopts the weathering steel composition provided by the present invention, and the process adopts low-temperature final rolling and low-temperature coiling process, the amount of water for centralized cooling is increased, the cooling rate is increased, and the microstructure of the weathering steel is granular bainite, such as Figure 3 As shown, the strength is higher, but the yield strength ratio, elongation and cold bending performance are poor.

[0047] In summary, the low-cost, easy-to-form hot-rolled high-weathering steel provided by the present invention has low alloy cost, easy-to-control production process, stable organizational performance, and can achieve stable batch industrial production. It can be widely used in the manufacture of stamping and roll-bending formed parts in industries such as railway vehicles, power towers, and container plates.

Claims

1. A low-cost, easy-to-form hot-rolled high-weathering steel, characterized in that: The chemical composition of the weathering steel is calculated by weight percentage as follows: C: 0.08-0.10, Si: 0.30-0.40, Mn: 0.40-0.50, P: 0.07-0.13, S≤0.006, Als: 0.020-0.030, Nb: 0.006-0.015, Ti: 0.008-0.018, Cu: 0.25-0.40, Cr: 0.35-0.75, Ni≤0.05, and the balance is Fe and unavoidable impurities; in addition, the chemical composition of the weathering steel also satisfies 810≤T≤820, wherein T=810+275[P]-21[Cu]-25[Cr]-36[Ni].

2. The low-cost, easy-to-form hot-rolled high-weathering steel according to claim 1, characterized in that: The thickness of the weathering steel is 2 to 8 mm.

3. The low-cost, easy-to-form hot-rolled high-weathering steel according to claim 1, characterized in that: The room temperature structure of the weathering steel is composed of ferrite and pearlite, wherein the ferrite content is 80-90%.

4. The low-cost, easy-to-form hot-rolled high-weathering steel according to claim 1, characterized in that: The weathering steel has a yield strength of 421-465 MPa, a tensile strength of 537-587 MPa, a yield strength ratio of 0.77-0.80, an elongation of 30-33.5%, and a 72h periodic immersion corrosion rate of ≤1.50 g / (m 2 h).

5. A method for producing low-cost, easy-to-form hot-rolled high-weathering steel according to any one of claims 1 to 4, characterized in that: It includes converter smelting, LF refining, continuous casting, billet heating, controlled rolling and cooling, and coiling processes.

6. The method for producing low-cost, easy-to-form hot-rolled high-weathering steel according to claim 5, characterized in that: In the casting billet heating process, the casting billet heating time is 150 to 200 minutes and the furnace discharge temperature is 1180 to 1210°C.

7. The method for producing low-cost, easy-to-form hot-rolled high-weathering steel according to claim 5, characterized in that: In the controlled rolling and controlled cooling process, the rough rolling outlet temperature is 1020-1050°C, the finishing rolling inlet temperature is 1000-1020°C, and the final rolling temperature is 880-910°C.

8. The method for producing low-cost, easy-to-form hot-rolled high-weathering steel according to claim 5, characterized in that: The controlled rolling and controlled cooling process has an average cooling rate of laminar cooling after rolling. CR Controlled at 20-25℃ / s, while the alloy element combination T and the average cooling rate of laminar cooling CR The secondary combination Ar3=T-6.2 CR Controlled between 660 and 690.

9. The method for producing low-cost, easy-to-form hot-rolled high-weathering steel according to claim 5, characterized in that: In the coiling process, the coiling temperature is 500-530°C.

Citation Information

Cited By

  • A weathering steel and a method for controlling the flatness of weathering steel coils