Method for improving anisotropy of near-alpha titanium alloy plate

Through vacuum consumable smelting and electron beam cold bed smelting combined with multi-fire commutation rolling and multi-pass cross-rolling, followed by multiple annealing, the poor moldability problem of near-α titanium alloy sheet due to strong texture is solved, significantly Improves its mechanical properties and uniformity.

CN118957466APending Publication Date: 2024-11-15CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411157801.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Due to its strong texture, the moldability of the near-α titanium alloy sheet is difficult to achieve uniform performance during processing.

Method used

Vacuum consumable smelting combined with electron beam cold bed smelting, multi-fire commutation rolling and multi-pass cross-rolling, followed by multiple annealing to reduce the anisotropy of the plate.

Benefits of technology

It effectively reduces the texture strength of titanium alloy sheets, improves its mechanical properties and corrosion resistance, improves molding performance, and achieves uniformity and efficient production of the sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957466A_ABST
    Figure CN118957466A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of titanium alloys. The invention discloses a method for improving anisotropy of a near-alpha titanium alloy plate. The method comprises the following steps: pressing raw materials into blocks to prepare a consumable electrode, and carrying out vacuum consumable smelting to obtain a titanium alloy cast ingot; the cast ingot is subjected to electron beam cold bed smelting, and a titanium alloy straight-rolled slab ingot is obtained; the slab ingot is heated to the first temperature higher than the beta phase transformation point temperature, heat preservation is conducted, then multi-heating-number reversing rolling is conducted, and a first slab is obtained; performing multi-pass cross rolling on the first plate blank to obtain a second plate blank; and the second plate blank is subjected to multiple annealing, and the near-alpha titanium alloy plate with improved anisotropy is obtained. According to the method disclosed by the invention, the texture strength of the near-alpha titanium alloy plate is reduced by optimizing alloy components and smelting and processing technologies, so that the near-alpha titanium alloy plate with improved anisotropy is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium alloys, and in particular to a method for improving the anisotropy of a near-alpha titanium alloy plate. Background Art

[0002] Titanium alloy plates have low density, high specific strength, excellent high and low temperature performance, and good corrosion resistance. They are important lightweight structural materials in aerospace, marine engineering, chemical industry, nuclear industry, etc. However, due to the importance of its application field, strict requirements are placed on the stability of titanium alloy performance, which puts forward higher requirements on the organization and performance control of each production link of titanium alloy materials.

[0003] There are mainly two types of crystal structures in titanium alloys: α phase and β phase. Titanium alloys can be divided into α-type titanium alloys, α+β-type titanium alloys and β-type titanium alloys according to the ratio of the two phases. Pure titanium and near-α-type titanium alloys are mainly composed of hexagonal close-packed α phase. At room temperature, the anisotropy of the unit cell of the near-α-type titanium alloy with a close-packed hexagonal crystal structure is very obvious. Titanium alloy plates are generally polycrystalline. Due to the low lattice symmetry and fewer independent slip systems, it is very easy to form a strong deformation texture during processing, and it is easy to generate recrystallization texture during annealing, causing anisotropy of properties such as elastic modulus, strength, plasticity, and toughness. The preferred orientation of texture or crystal is one of the important reasons for the anisotropy of polycrystalline material properties. For near-α-type titanium alloys, which are close-packed hexagonal metals with low symmetry and fewer slip systems, it is very easy to form textures during processing, causing problems such as "earing" during stamping and scrapping of the plate. In order to improve the processing and forming properties of the plate, it is hoped that the near-α-type titanium alloy plate has the minimum plate surface anisotropy.

[0004] Therefore, how to reduce the texture strength of near-α titanium alloy sheets has become an urgent problem to be solved in this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for improving the anisotropy of a near-α titanium alloy plate, so as to solve the problem that the existing near-α titanium alloy plate has poor plate formability due to its strong texture.

[0006] According to one aspect of the present invention, there is provided a method for improving the anisotropy of a near-α titanium alloy plate, comprising the following steps: Step S1: pressing the raw material into blocks to prepare consumable electrodes for vacuum consumable melting to obtain titanium alloy ingots; Step S2: subjecting the ingot to electron beam cold-bed melting to obtain a titanium alloy direct-rolled flat ingot, wherein the flat ingot comprises the following components by weight percentage: Mo: 0.2%-0.5%, Ni: 0.6%-0.9%, Cr: 0.6%-0.8%, Sc: 0.15%-0.2%, and the balance is Ti and unavoidable impurities; Step S3: heating the flat ingot to a first temperature higher than the β phase transformation point temperature and maintaining the temperature, and then performing multiple heat reversing rolling to obtain a first slab; Step S4: performing multiple cross-rolling on the first slab to obtain a second slab; Step S5: performing multiple annealing on the second slab to obtain a near-α titanium alloy plate with improved anisotropy.

[0007] According to one embodiment of the present invention, the raw materials include: 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder.

[0008] According to one embodiment of the present invention, the vacuum consumable smelting is performed twice, and the vacuum degree is maintained below 2.0 Pa during smelting, and the ingot from each smelting is turned around before the next smelting.

[0009] According to one embodiment of the present invention, the first temperature is 50-100° C. above the β phase transition point temperature, and the insulation time is 3-5 hours.

[0010] According to one embodiment of the present invention, the multi-pass reversing rolling is a two-pass reversing rolling, the first pass adopts transverse hot rolling, the second pass hot rolling direction is perpendicular to the first pass hot rolling direction, and after each rolling pass is completed, the slab is straightened, corrected, acid-alkali cleaned and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0011] According to one embodiment of the present invention, the deformation amount of the first hot rolling pass is controlled at 20% to 30%.

[0012] According to one embodiment of the present invention, the deformation amount of the second hot rolling pass is controlled at 10% to 20%.

[0013] According to one embodiment of the present invention, in the multiple-pass cross-rolling, the pass deformation is controlled at 5% to 10%, and the slab is synchronously rolled in the horizontal direction. After each rolling pass, the slab is rotated 15 to 30° clockwise in the horizontal plane relative to its feed direction before the next rolling pass, and the total deformation is controlled at 60% to 80%.

[0014] According to one embodiment of the present invention, step S4 further includes: After each rolling process except the last one, the slab is straightened, corrected, cleaned with acid and alkali, and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0015] According to one embodiment of the present invention, the multiple annealing in step S5 includes: Step S5-1: heating the cold-rolled sheet to a temperature 50-100°C above the β phase transformation point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a primary annealed sheet; Step S5-2: heating the primary annealing sheet to 50-100° C. below the β phase transition point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a secondary annealing sheet; Step S5-3: heating the secondary annealed sheet to a temperature 50-100° C. above the α / β phase transition point and keeping the temperature for 1-2 hours, then cooling the sheet to room temperature to obtain a near-α titanium alloy sheet with improved anisotropy; Among them, the heating rate of each annealing is 10~15℃ / min.

[0016] Compared with the prior art, the present invention has the following advantages: (1) The combination of vacuum autoclave (VAR) smelting and EB furnace smelting can directly produce rectangular ingots for direct rolling, which can not only save the forging step, greatly reduce the cost of billet opening, effectively shorten the preparation process, and improve the preparation efficiency, but also can well solve the problems of high and low density inclusions in the smelting process of titanium and titanium alloys, and easily realize the mass production of titanium alloy plates; (2) Adding an appropriate amount of rare earth element Sc to near-α titanium alloy can refine the metal material grains and greatly improve the mechanical properties of the alloy. Adding a certain amount of Cr can simultaneously improve the mechanical properties and corrosion resistance of the alloy; (3) The reversing hot rolling and multi-pass reversing cold rolling technology were used to promote the formation of base surface texture in the titanium plate, which is beneficial to reduce the anisotropy of the plate and improve the mechanical properties of the titanium plate; (4) After cold rolling, multiple annealing heat treatment is used to produce a certain redistribution of texture orientation, so that the anisotropy is improved, thereby obtaining a near-α titanium alloy plate with better mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.

[0018] Figure 1A flow chart of a method for improving anisotropy of a near-α titanium alloy plate according to an embodiment of the present invention; Figure 2 is a texture diagram of a finished plate prepared according to the method of Example 1; Figure 3 This is the texture diagram of the finished plate prepared according to the method of Example 2. DETAILED DESCRIPTION

[0019] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0020] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.

[0021] It should be understood that the embodiments of the present invention shown in the exemplary embodiments are only illustrative. Although only a few embodiments are described in detail in the present invention, it is easy for those skilled in the art to appreciate that multiple modifications are feasible without actually departing from the teaching of the subject matter of the present invention. Accordingly, all such modifications should be included within the scope of the present invention. Without departing from the gist of the present invention, other replacements, modifications, changes and deletions may be made to the design, operating conditions and parameters of the following exemplary embodiments.

[0022] According to one aspect of the present invention, a method for improving the anisotropy of a near-α titanium alloy plate is provided. Figure 1 As shown, the method generally comprises the following steps: Step S1: pressing the raw material into blocks to prepare consumable electrodes for vacuum consumable melting to obtain titanium alloy ingots; Step S2: subjecting the ingot to electron beam cold-bed melting to obtain a titanium alloy direct-rolled flat ingot, wherein the flat ingot comprises the following components by weight percentage: Mo: 0.2%-0.5%, Ni: 0.6%-0.9%, Cr: 0.6%-0.8%, Sc: 0.15%-0.2%, and the remainder is Ti and unavoidable impurities; Step S3: heating the flat ingot to a first temperature higher than the β phase transformation point temperature and maintaining the temperature, and then performing multiple heat reversing rolling to obtain a first slab; Step S4: performing multiple cross-rolling on the first slab to obtain a second slab; Step S5: performing multiple annealing on the second slab to obtain a near-α titanium alloy plate with improved anisotropy.

[0023] The various operating steps of the method for improving the anisotropy of the near-α titanium alloy plate of the present invention are described in detail below.

[0024] In step S1, the raw materials are pressed into blocks to prepare consumable electrodes for vacuum consumable melting to obtain titanium alloy ingots. In some embodiments, the raw materials include: 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder. In some embodiments, vacuum consumable melting is performed twice, and the vacuum degree is maintained below 2.0 Pa during melting, and the ingots of each melting are turned around for the next melting.

[0025] For example, 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder can be mixed according to the composition of the target titanium alloy to be prepared, pressed into blocks, and welded together to make consumable electrodes. The test ingots are vacuum melted twice, and the vacuum degree is maintained below 2.0 Pa. The ingots from each melt are turned around for the next melt.

[0026] In step S2, the ingot is subjected to electron beam cold hearth melting to obtain a titanium alloy direct-rolled flat ingot, wherein the flat ingot comprises the following components by weight percentage: Mo: 0.2%~0.5%, Ni: 0.6%~0.9%, Cr: 0.6%~0.8%, Sc: 0.15%~0.2%, and the remainder is Ti and unavoidable impurities.

[0027] For example, the ingot can be placed in a 200-250kW electron beam cooling furnace for a single smelting, and after milling and grinding, a large-sized long rectangular near-α titanium alloy direct-rolled flat ingot with a thickness of 150-200mm can be obtained.

[0028] In the above steps, the combination of vacuum autoclave (VAR) smelting and EB furnace smelting can directly produce rectangular ingots for direct rolling, which can not only save the forging step, greatly reduce the cost of billet opening, effectively shorten the preparation process, and improve the preparation efficiency, but also can well solve the problems of high and low density inclusions in the smelting process of titanium and titanium alloys, and easily realize the mass production of titanium alloy plates. Adding an appropriate amount of rare earth element Sc to near-α titanium alloy can refine the grains of metal materials and greatly improve the mechanical properties of the alloy. Compound addition of a certain amount of Cr can simultaneously improve the mechanical properties and corrosion resistance of the alloy.

[0029] In step S3, the flat ingot is heated to a first temperature higher than the β phase transformation point temperature and kept warm, and then subjected to multiple heat reversing rolling to obtain a first slab.

[0030] In some embodiments, the first temperature is 50-100° C. above the β phase transition point temperature, and the holding time is 3-5 hours.

[0031] In some embodiments, the multi-pass reversing rolling is a two-pass reversing rolling, wherein the first pass is transverse hot rolling, and the second pass is hot rolling in a direction perpendicular to the first pass. After each rolling pass, the slab is straightened, corrected, acid-alkali cleaned, and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0032] In some embodiments, the deformation amount of the first hot rolling pass is controlled at 20% to 30%, and the deformation amount of the second hot rolling pass is controlled at 10% to 20%.

[0033] For example, the obtained straight-rolled flat ingot can be cut into several blocks of suitable specifications, and the blocks are heated to 50~100℃ above the β phase transformation point temperature. Then two rounds of reversing hot rolling are carried out. The first round adopts transverse hot rolling, and the deformation of the pass is controlled at 20%~30%, and the thickness of the obtained plate is 15~30mm; the hot rolling direction of the second round is perpendicular to the hot rolling direction of the first round, and the deformation of the pass is controlled at 10%~20%, and the thickness of the obtained plate is 5~10mm. Before each rolling, the slab is heated to 50~100℃ above the β phase transformation point temperature. After each rolling, the slab is straightened, corrected, acid-base cleaned and ground, and then placed in a vacuum annealing furnace for 1.5~2h annealing at 650~700℃, and then the furnace is cooled to room temperature.

[0034] In step S4, the first slab is subjected to multiple cross-rolling passes to obtain a second slab.

[0035] In some embodiments, in multiple-pass cross-rolling, the deformation of each pass is controlled at 5% to 10%, and the slab is rolled synchronously in the horizontal direction. After each rolling pass, the slab is rotated 15 to 30° clockwise in the horizontal plane relative to its feed direction before the next rolling pass, and the total deformation is controlled at 60% to 80%.

[0036] In some embodiments, after each rolling pass except the last one, the slab is straightened, corrected, cleaned with acid and alkali, and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0037] For example, the first slab can be cross-rolled for multiple passes, the deformation of the cold rolling pass is controlled at 5%~10%, and it is synchronously rolled in the horizontal direction. After each rolling pass, the billet is rotated 15~30° clockwise in the horizontal plane relative to its feed direction before the next rolling pass. The total deformation is 60%~80%, and the thickness of the resulting titanium plate is 2~3mm. In addition to the finished plate, after each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then placed in a vacuum annealing furnace for 1.5~2 hours at 700~750℃, and the furnace is cooled to room temperature.

[0038] In the above operation, reversing hot rolling and multi-pass reversing cold rolling technology are used to promote the generation of base surface texture in the titanium plate, which is beneficial to weaken the anisotropy of the plate and improve the mechanical properties of the titanium plate.

[0039] In step S5, the second slab is subjected to multiple annealing to obtain a near-α titanium alloy plate with improved anisotropy.

[0040] In some embodiments, the multiple annealing comprises: Step S5-1: heating the cold-rolled sheet to a temperature 50-100°C above the β phase transformation point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a primary annealed sheet; Step S5-2: heating the primary annealing sheet to 50-100°C below the β phase transition point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a secondary annealing sheet; Step S5-3: heating the secondary annealed sheet to 50-100° C. above the α / β phase transition point temperature and keeping the temperature for 1-2 hours, then cooling the sheet to room temperature to obtain a near-α titanium alloy sheet with improved anisotropy; Among them, the heating rate of each annealing is 10~15℃ / min.

[0041] For example, the cold-rolled sheet can be heated to 50~100℃ above the β phase transition point temperature, kept for 1~2 hours, and then furnace cooled to room temperature; then the cold-rolled sheet can be heated to 50~100℃ below the β phase transition point temperature, kept for 1-2 hours, and then furnace cooled to room temperature; finally, the cold-rolled sheet can be heated to 50~100℃ above the α / β phase transition point temperature, kept for 1~2 hours, and then furnace cooled to room temperature. The heating rate used is 10~15℃ / min, and a near-α titanium alloy sheet with weak anisotropy is obtained.

[0042] In the above operation, multiple annealing heat treatment is used after cold rolling deformation to produce a certain redistribution of texture orientation, so that the anisotropy is improved, thereby obtaining a near-α titanium alloy plate with better mechanical properties.

[0043] The technical solution of the present invention will be further described below by specific examples. Unless otherwise specified, the raw materials, equipment, consumables, etc. used in the following examples can be obtained by conventional commercial means, and the pole figure testing method used is a conventional testing method in the art.

[0044] Example 1 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder are used as raw materials, and the prepared ingot includes the following weight percentages: Mo: 0.5%, Ni: 0.8%, Cr: 0.6%, Sc: 0.18%, and the remainder is Ti and unavoidable impurities, wherein the impurity elements range from Fe≤0.3%, C≤0.08%, N≤0.03%, H≤0.01%, and O≤0.25%. After the raw materials are mixed, they are pressed into blocks by a briquetting machine, and each block is welded together to form a consumable electrode. The experimental ingot is vacuum smelted twice, and the vacuum degree is maintained below 2.0Pa. The ingot of each smelting is turned around for the next smelting.

[0045] The ingot after the two smeltings was placed in a 250kW electron beam cooling furnace for a second smelting. After milling and grinding, a large-sized long rectangular near-α titanium alloy direct-rolled flat ingot with a thickness of 150mm was obtained.

[0046] The obtained straight-rolled flat ingot is cut into several blocks of suitable specifications, and the blocks are heated to 950℃ and kept warm for 4 hours. Then two rounds of reversing hot rolling are carried out. The first round adopts transverse hot rolling, and the deformation of each pass is controlled at 20%~30%, and the thickness of the obtained plate is 15mm; the hot rolling direction of the second round is perpendicular to the hot rolling direction of the first round, and the deformation of each pass is controlled at 10%~20%, and the thickness of the obtained plate is 6mm. After each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then placed in an annealing furnace at 650℃ for 2 hours, and the furnace is cooled to room temperature.

[0047] Then, multiple cross-rolling passes are carried out, and the deformation of the cold rolling pass is controlled at 5%~10%. It is rolled synchronously in the horizontal direction. After each rolling pass, the billet is rotated 15° clockwise in the horizontal plane relative to its feed direction before the next rolling pass. The total deformation is 60%, and the thickness of the obtained titanium plate is 2mm. Except for the finished plate, after each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then annealed at 700℃ for 2 hours in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0048] Finally, triple annealing is performed, and the specific operation is to first heat the cold-rolled plate to 950℃ for 2h, then cool it to room temperature in the furnace, then heat the cold-rolled plate to 850℃ for 1h, then cool it to room temperature in the furnace, and finally heat the cold-rolled plate to 950℃ for 2h, then cool it to room temperature in the furnace. The heating rate is 10℃ / min. The slab is straightened, corrected, acid-base cleaned and ground to obtain a near-α titanium alloy plate with improved anisotropy.

[0049] Figure 2The texture diagram of the finished plate prepared according to the method of this embodiment is shown. After testing, the plate texture consists of basal ND texture, basal double peak and a certain amount of basal TD texture, and the texture strength is low. Samples were taken for performance testing. The transverse performance: tensile strength is 496MPa, yield strength is 374MPa, and elongation is 17.6%; longitudinal performance: tensile strength is 489MPa, yield strength is 368MPa, and elongation is 17.8%, indicating that the product is uniform and has no obvious anisotropy.

[0050] Example 2 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder are used as raw materials, and the prepared ingot includes the following weight percentages: Mo: 0.4%, Ni: 0.9%, Cr: 0.6%, Sc: 0.2%, and the remainder is Ti and unavoidable impurities, wherein the impurity elements range from Fe≤0.3%, C≤0.08%, N≤0.03%, H≤0.01%, O≤0.25%. After the raw materials are mixed, they are pressed into blocks by a briquetting machine, and each block is welded together to form a consumable electrode. The experimental ingot is vacuum smelted twice, and the vacuum degree is maintained below 2.0Pa. The ingot of each smelting is turned around for the next smelting.

[0051] The ingot after the two smeltings was placed in a 200kW electron beam cooling furnace for a second smelting. After milling and grinding, a large-sized long rectangular near-α titanium alloy direct-rolled flat ingot with a thickness of 180 mm was obtained.

[0052] The obtained straight-rolled flat ingot is cut into several blocks of suitable specifications, and the blocks are heated to 980℃ and kept warm for 3 hours. Then two rounds of reversing hot rolling are carried out. The first round adopts transverse hot rolling, and the deformation of each pass is controlled at 20%~30%, and the thickness of the obtained plate is 24mm; the hot rolling direction of the second round is perpendicular to the hot rolling direction of the first round, and the deformation of each pass is controlled at 10%~20%, and the thickness of the obtained plate is 5mm. After each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then placed in an annealing furnace at 680℃ for 2 hours, and the furnace is cooled to room temperature.

[0053] Then, multiple cross-rolling passes are carried out, and the deformation of the cold rolling pass is controlled at 5%~10%. It is rolled synchronously in the horizontal direction. After each rolling pass, the billet is rotated 30° clockwise in the horizontal plane relative to its feed direction before the next rolling pass. The total deformation is 80%, and the thickness of the obtained titanium plate is 2.5mm. Except for the finished plate, after each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then annealed at 750℃ for 1.5 hours in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0054] Finally, triple annealing is performed, and the specific operation is to first heat the cold-rolled plate to 980℃ for 2h, then furnace cool to room temperature, then heat the cold-rolled plate to 800℃ for 1h, then furnace cool to room temperature, and finally heat the cold-rolled plate to 950℃ for 2h, then furnace cool to room temperature. The heating rate is 15℃ / min. The slab is straightened, corrected, acid-base cleaned and ground to obtain a near-α titanium alloy plate with improved anisotropy.

[0055] Figure 3 The texture diagram of the finished plate prepared according to the method of this embodiment is shown. After testing, the plate texture consists of basal ND texture, basal double peak and a certain amount of basal TD texture, and the texture strength is low. Sampling was performed for performance testing. The transverse performance: tensile strength is 484MPa, yield strength is 362MPa, and elongation is 17.9%; longitudinal performance: tensile strength is 477MPa, yield strength is 358MPa, and elongation is 18.2%, indicating that the product is uniform and has no obvious anisotropy.

[0056] Example 3 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder are used as raw materials, and the prepared ingot includes the following weight percentages: Mo: 0.2%, Ni: 0.6%, Cr: 0.8%, Sc: 0.15%, and the remainder is Ti and unavoidable impurities, wherein the impurity elements range from Fe≤0.3%, C≤0.08%, N≤0.03%, H≤0.01%, and O≤0.25%. After the raw materials are mixed, they are pressed into blocks by a briquetting machine, and each block is welded together to form a consumable electrode. The experimental ingot is vacuum smelted twice, and the vacuum degree is maintained below 2.0Pa. The ingot of each smelting is turned around for the next smelting.

[0057] The ingot after the two smeltings was placed in a 200kW electron beam cooling furnace for a second smelting. After milling and grinding, a large-sized long rectangular near-α titanium alloy direct-rolled flat ingot with a thickness of 180 mm was obtained.

[0058] The obtained straight-rolled flat ingot is cut into several blocks of suitable specifications, and the blocks are heated to 960℃ and kept warm for 5 hours. Then two rounds of reversing hot rolling are carried out. The first round adopts transverse hot rolling, and the deformation of each pass is controlled at 20%~30%, and the thickness of the obtained plate is 22mm; the hot rolling direction of the second round is perpendicular to the hot rolling direction of the first round, and the deformation of each pass is controlled at 10%~20%, and the thickness of the obtained plate is 5mm. After each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then placed in an annealing furnace at 680℃ for 2 hours, and the furnace is cooled to room temperature.

[0059] Then, multiple cross-rolling passes are carried out, and the deformation of the cold rolling pass is controlled at 5%~10%. It is rolled synchronously in the horizontal direction. After each rolling pass, the billet is rotated 25° clockwise in the horizontal plane relative to its feed direction before the next rolling pass. The total deformation is 70%, and the thickness of the obtained titanium plate is 2mm. Except for the finished plate, after each rolling pass, the slab is straightened, corrected, acid-base cleaned and ground, and then annealed at 680℃ for 2 hours in a vacuum annealing furnace, and the furnace is cooled to room temperature.

[0060] Finally, triple annealing is performed, and the specific operation is to first heat the cold-rolled plate to 960℃ for 2h, then furnace cool to room temperature, then heat the cold-rolled plate to 860℃ for 1h, then furnace cool to room temperature, and finally heat the cold-rolled plate to 960℃ for 2h, then furnace cool to room temperature. The heating rate is 10℃ / min. The slab is straightened, corrected, acid-base cleaned and ground to obtain a near-α titanium alloy plate with improved anisotropy.

[0061] Sampling was carried out for performance testing. The transverse performance was as follows: tensile strength was 486MPa, yield strength was 365MPa, and elongation was 17.8%; the longitudinal performance was as follows: tensile strength was 479MPa, yield strength was 358MPa, and elongation was 18.1%, indicating that the product is uniform and has no obvious anisotropy.

[0062] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention is limited to these examples; under the idea of ​​the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for improving the anisotropy of a near-α titanium alloy plate, characterized in that: The following steps are involved: Step S1: pressing the raw material into blocks to prepare consumable electrodes for vacuum consumable melting to obtain titanium alloy ingots; Step S2: subjecting the ingot to electron beam cold-bed melting to obtain a titanium alloy direct-rolled flat ingot, wherein the flat ingot comprises the following components by weight percentage: Mo: 0.2%-0.5%, Ni: 0.6%-0.9%, Cr: 0.6%-0.8%, Sc: 0.15%-0.2%, and the balance is Ti and unavoidable impurities; Step S3: heating the flat ingot to a first temperature higher than the β phase transformation point temperature and maintaining the temperature, and then performing multiple heat reversing rolling to obtain a first slab; Step S4: performing multiple cross-rolling on the first slab to obtain a second slab; Step S5: performing multiple annealing on the second slab to obtain a near-α titanium alloy plate with improved anisotropy.

2. The method for improving the anisotropy of a near-α titanium alloy plate according to claim 1, characterized in that: The raw materials include: 0A grade titanium sponge, Ti-15Mo master alloy, pure nickel chips, elemental chromium and scandium powder.

3. The method for improving the anisotropy of a near-α titanium alloy plate according to claim 1, characterized in that: The vacuum consumable smelting is performed twice, and the vacuum degree is maintained below 2.0 Pa during smelting, and the ingot from each smelting is turned around for the next smelting.

4. The method for improving anisotropy of a near-α titanium alloy plate according to claim 1, characterized in that: The first temperature is 50-100° C. above the β phase transition point temperature, and the insulation time is 3-5 hours.

5. The method for improving anisotropy of near-α titanium alloy plate according to claim 1, characterized in that: The multi-pass reversing rolling is a two-pass reversing rolling, wherein the first pass adopts transverse hot rolling, and the hot rolling direction of the second pass is perpendicular to the hot rolling direction of the first pass. After each rolling pass is completed, the slab is straightened, corrected, acid-alkali cleaned and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

6. The method for improving the anisotropy of a near-α titanium alloy plate according to claim 5, characterized in that: The deformation of the first hot rolling pass is controlled at 20%~30%.

7. The method for improving anisotropy of a near-α titanium alloy plate according to claim 5, characterized in that: The deformation of the second hot rolling pass is controlled at 10%~20%.

8. The method for improving anisotropy of a near-α titanium alloy plate according to claim 1, characterized in that: In the multi-pass cross rolling, the pass deformation is controlled at 5% to 10%, and the slab is synchronously rolled in the horizontal direction. After each rolling pass, the slab is rotated 15 to 30° clockwise in the horizontal plane relative to its feed direction before the next rolling pass, and the total deformation is controlled at 60% to 80%.

9. The method for improving anisotropy of a near-α titanium alloy plate according to claim 8, characterized in that: The step S4 further comprises: After each rolling process except the last one, the slab is straightened, corrected, cleaned with acid and alkali, and ground, and then annealed in a vacuum annealing furnace, and the furnace is cooled to room temperature.

10. The method for improving anisotropy of a near-α titanium alloy plate according to claim 1, characterized in that: The multiple annealing in step S5 includes: Step S5-1: heating the cold-rolled sheet to a temperature 50-100°C above the β phase transformation point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a primary annealed sheet; Step S5-2: heating the primary annealing sheet to 50-100° C. below the β phase transition point and keeping the temperature for 1-2 hours, then cooling the furnace to room temperature to obtain a secondary annealing sheet; Step S5-3: heating the secondary annealed sheet to a temperature 50-100° C. above the α / β phase transition point and keeping the temperature for 1-2 hours, then cooling the sheet to room temperature to obtain a near-α titanium alloy sheet with improved anisotropy; Among them, the heating rate of each annealing is 10~15℃ / min.

Citation Information

Cited By

  • Thermal mechanical treatment method of TC4B titanium alloy for armor

    CN119794076A

  • Method for reducing anisotropy of continuous annealing alpha-phase titanium plate and titanium plate