PVD (Physical Vapor Deposition) preparation method of transparent silicon dioxide film
By using anode layer ion source to improve oxygen ionization rate and oxygen ion energy in the PVD preparation method, the problem of low transparency of traditional silica films is solved, and a high transparency silicon dioxide film preparation is achieved, suitable for anti-fingerprint coatings , significantly reduces the color discoloration amplitude of the product.
Patent Information
- Application Number
- CN202411073414.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
AI Technical Summary
In the traditional silicon dioxide thin film PVD preparation method, the low oxygen ionization rate and insufficient oxygen ion energy lead to low transparency of the resulting film, affecting the transparency of the anti-fingerprint coating and the color change amplitude of the product appearance.
Anode layer ion source is used to increase the oxygen ionization rate and oxygen ion energy, and the yield and transparency of silica are significantly improved by reacting with the oxygen ion flow of the silicon target.
It significantly improves the transparency of the silicon dioxide film, reduces the color discoloration amplitude of the product, and makes the transparency reach more than 90% of the glass substrate material, and is suitable for anti-fingerprint coatings.
Smart Images

Figure CN118957512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PVD coating, and in particular relates to a PVD preparation method of a transparent silicon dioxide film. Background Art
[0002] Anti-fingerprint coating (AF), also known as anti-fingerprint coating, is a nanostructured material developed by imitating the self-cleaning effect of lotus leaves to resist oil and fingerprints on the surface of materials. Anti-fingerprint coating is suitable for the surface of glass, ceramics, metals, plastics and other materials. It can improve the hydrophobicity and oleophobicity of the material, making it waterproof, oil-proof, anti-fouling, anti-fingerprint adhesion and other functions, improve its easy cleaning, and has the advantages of improving the smoothness and wear resistance of the material.
[0003] The most commonly used material for anti-fingerprint coatings is silicon surface fluorine material, which is composed of two functional groups: low surface energy fluorinated groups and surface reactive groups. When the organic fluoride contacts the surface of the material, the surface reactive group will chemically react with the corresponding surface functional group to produce chemical bonds and then form a film. The main reactive group of the self-limiting organic fluoride is a condensation reaction with the hydroxyl group (Si-OH) on the surface of the deposited glass (the main component is SiO2), but there is no Si-OH on the metal surface of the mobile phone. Therefore, if such organic fluoride is to be used on metal or other materials, a layer of SiO2 must be plated on the surface of the metal or material, and then a low surface energy organic fluoride must be plated. Therefore, improving the transparency of the SiO2 film, that is, increasing the proportion of SiO2 in the film, helps to reduce the degree of discoloration of the product appearance caused by the anti-fingerprint film.
[0004] However, in the PVD preparation method of the transmitted silicon dioxide film, a mixture of oxygen and argon is introduced into a vacuum chamber for direct reactive sputtering. The ionization rate of oxygen is very low, and the energy of oxygen ions is low. The probability of silicon atoms reacting with oxygen after being sputtered out of the target is low. The proportion of transparent silicon dioxide in the generated film is small, and the proportion of opaque pure silicon is large. Therefore, the transparency of the film is low. As a part of the AF film (silicon dioxide + organic fluoride), the product changes color greatly after AF coating. Summary of the invention
[0005] To solve the above problems, the present invention aims to provide a PVD preparation method for a transparent silicon dioxide film, which uses an anode layer ion source to increase the oxygen ionization rate and oxygen ion energy, increase the sputtering yield of silicon dioxide, and thus improve the transparency of the anti-fingerprint film.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] The present invention provides a PVD preparation method for a transparent silicon dioxide film, comprising the steps of:
[0008] S1: Fix the substrate material in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber;
[0009] S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value;
[0010] S3: Turn on the bias power supply, set the voltage and duty cycle, and perform glow cleaning on the surface of the substrate material;
[0011] S4: adjust the bias voltage and introduce oxygen from the ion source to make the gas pressure in the furnace reach a specific value;
[0012] S5: Start the ion source and switch to the constant voltage mode. After the ion source works stably for a period of time, start the silicon target power supply to start the coating;
[0013] S6: First turn off the power of the silicon target and ion source, then turn off the oxygen and argon gases to end the coating.
[0014] Furthermore, the substrate material in step S1 is a material that needs to be coated with a transparent silicon dioxide film, and the vacuum chamber is heated and maintained at 150°C.
[0015] Furthermore, in step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
[0016] Further, in step S3, the voltage is set to 300V, the duty cycle is set to 50%, and glow cleaning is performed for 15-20 minutes to remove dust and oxides on the surface of the substrate material;
[0017] Furthermore, in step S4, the bias voltage is set to 100V, and the specific value of the gas pressure in the furnace is 0.5Pa.
[0018] Furthermore, in step S5, the voltage of the constant voltage mode is set to 900V.
[0019] Further, in step S5, after the ion source has been working stably for 1 minute, the silicon target power supply is started, the current is set to 8-12A, the silicon target voltage is reduced to 270-330V, and the coating is performed for 10 minutes.
[0020] Furthermore, in the PVD preparation method, the target material is configured as: a pair of silicon targets and an anode layer ion source; wherein the anode layer ion source is installed on the side of the silicon target, and the silicon target is sputtered by argon ions to produce silicon atoms or ions, which are more easily reacted with the oxygen ion flow ejected from the side ion source to generate silicon dioxide deposition and the substrate surface.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: the ionization rate of oxygen is increased through the ion source, and a higher energy oxygen ion beam is generated to act on the glow area of the adjacent silicon target sputtering. The probability of collision and chemical reaction between silicon atoms or silicon ions generated by the silicon target sputtering and oxygen ions is significantly increased, and the silicon and oxygen combination rate is significantly improved, thereby significantly increasing the yield of silicon dioxide and correspondingly reducing the production of pure silicon. Therefore, the plated silicon dioxide film has a higher transparency and can significantly reduce the color change of the product when applied to AF. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a flowchart of the preparation method of this embodiment. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0024] To achieve the above object, the technical solution of the present invention is as follows:
[0025] See also Figure 1 As shown, this embodiment provides a PVD preparation method for a transparent silicon dioxide film, wherein the target material is configured as: a pair of silicon targets, and an anode layer ion source is configured; wherein the anode layer ion source is installed on the side of the silicon target, and the coating method includes the following steps:
[0026] S1: Fix the stainless steel sheet or glass sheet as the base material in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber;
[0027] S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value;
[0028] S3: Turn on the bias power supply, set the voltage and duty cycle, and perform glow cleaning on the surface of the substrate material;
[0029] S4: adjust the bias voltage and introduce oxygen from the ion source to make the gas pressure in the furnace reach a specific value;
[0030] S5: Start the ion source and switch to the constant voltage mode. After the ion source works stably for a period of time, start the silicon target power supply to start the coating;
[0031] S6: First turn off the power of the silicon target and ion source, then turn off the oxygen and argon gases to end the coating.
[0032] Furthermore, in the present application, the anode layer ion source is installed on the side of the silicon target, and the silicon target is sputtered by argon ions to produce silicon atoms or ions, which are more likely to react with the oxygen ion flow ejected by the side ion source to generate silicon dioxide deposition on the substrate surface.
[0033] Furthermore, the substrate material in step S1 is a material that needs to be coated with a transparent silicon dioxide film, and the vacuum chamber is heated and maintained at 150°C.
[0034] Furthermore, in step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
[0035] Further, in step S3, the voltage is set to 300V, the duty cycle is set to 50%, and glow cleaning is performed for 15-20 minutes to remove dust and oxides on the surface of the substrate material;
[0036] Furthermore, in step S4, the bias voltage is set to 100V, and the specific value of the gas pressure in the furnace is 0.5Pa.
[0037] Furthermore, in step S5, the voltage of the constant voltage mode is set to 900V.
[0038] Further, in step S5, after the ion source has been working stably for 1 minute, the silicon target power supply is started, the current is set to 8-12A, the silicon target voltage is reduced to 270-330V, and the coating is performed for 10 minutes.
[0039] Further, in the PVD preparation method,
[0040] Compared with the prior art, the beneficial effects of the present invention are: the ionization rate of oxygen is increased through the ion source, and a high-energy oxygen ion beam is generated to act on the glow area of the adjacent silicon target sputtering. The probability of collision and chemical reaction between silicon atoms or silicon ions generated by the silicon target sputtering and oxygen ions is significantly increased, and the silicon and oxygen combination rate is significantly improved, thereby significantly increasing the production of silicon dioxide and correspondingly reducing the production of pure silicon. Therefore, the plated silicon dioxide film has a high transparency. It is found through measurement that the average transmittance of visible light can reach more than 90% of the glass substrate material. When applied to AF, the color change of the product can be significantly reduced.
[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A PVD preparation method for a transparent silicon dioxide film, characterized in that: Includes steps: S1: Fix the substrate material in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber; S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value; S3: Turn on the bias power supply, set the voltage and duty cycle, and perform glow cleaning on the surface of the substrate material; S4: adjust the bias voltage and introduce oxygen from the ion source to make the gas pressure in the furnace reach a specific value; S5: Start the ion source and switch to the constant voltage mode. After the ion source works stably for a period of time, start the silicon target power supply to start the coating; S6: First turn off the power of the silicon target and ion source, then turn off the oxygen and argon gases to end the coating.
2. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: The base material in step S1 is a material that needs to be coated with a transparent silicon dioxide film, and the vacuum chamber is heated and kept at 150°C.
3. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
4. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In step S3, the voltage is set to 300V, the duty cycle is set to 50%, and glow cleaning is performed for 15-20 minutes to remove dust and oxides on the surface of the substrate material.
5. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In step S4, the bias voltage is set to 100V, and the specific value of the gas pressure in the furnace is set to 0.5Pa.
6. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In step S5, the voltage of the constant voltage mode is set to 900V.
7. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In step S5, after the ion source has been working stably for 1 minute, the silicon target power supply is started, the current is set to 8-12A, the silicon target voltage is reduced to 270-330V, and the coating is carried out for 10 minutes.
8. The PVD preparation method of a transparent silicon dioxide film according to claim 1, characterized in that: In the PVD preparation method, the target material is configured as: a pair of silicon targets and an anode layer ion source; wherein the anode layer ion source is installed on the side of the silicon target, and the silicon target is sputtered by argon ions to produce silicon atoms or ions, which are more easily reacted with the oxygen ion flow ejected from the side ion source to generate silicon dioxide deposited on the surface of the substrate.
Citation Information
Cited By
Method for modifying the surface of stainless steel against microbiologically influenced corrosion
CN122833413A