Nanometer multilayer gradient heterogeneous composite coating and preparation method and application thereof

Through the design of AlCrN-AlCrN/TiSiN-AlCrTiSiN-TiSiN nano multilayer gradient heterogeneous composite coating, the problem of insufficient corrosion resistance of existing PVD coatings in HCl strong corrosion environment is solved, and high film-based binding force is achieved And the improvement of corrosion resistance, it is suitable for PVC injection molds and other applications.

CN119020734AActive Publication Date: 2024-11-26GUANGDONG UNIV OF TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411113949.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing PVD coatings have insufficient corrosion resistance in HCl-corrosive environments. The single structural coating has the problem of high binding force but easy to corrode, large internal stress in nano-multi-layer structures and reasonable thickness, resulting in coating peeling.

Method used

AlCrN-AlCrN/TiSiN-AlCrTiSiN-TiSiN nano multi-layer gradient heterogeneous composite coating is adopted. Through the composite of four coatings with different hardness, the gradient structure is designed, the film-based binding force and corrosion resistance are improved, and the high-density layer is introduced. The interface inhibits the penetration of corrosive media and regulates the thickness to improve corrosion resistance.

Benefits of technology

It achieves high film-based binding force and corrosion resistance, significantly improves the corrosion resistance of PVC injection molds and other products, extends the service life of the mold and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020734A_ABST
    Figure CN119020734A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano multilayer composite coatings, in particular to a nano multilayer gradient heterogeneous composite coating as well as a preparation method and application thereof. The nanometer multilayer gradient heterogeneous composite coating comprises an AlCrN bottom layer, an AlCrN / TiSiN nanometer multilayer, an AlCrTiSiN high-entropy layer and a TiSiN top layer which are arranged in sequence. Wherein the AlCrN / TiSiN nano multilayer is composed of AlCrN sub-layers and TiSiN sub-layers, the AlCrN sub-layers and the TiSiN sub-layers are alternately arranged, and the AlCrN sub-layers, the AlCrN bottom layer and the AlCrTiSiN high-entropy layer are connected. According to the invention, four coatings with different hardness are compounded, so that the defects of a coating with a single structure are overcome, the binding force between the coating and a matrix and other properties are improved, and the coating has high hardness, film-matrix binding force and corrosion resistance, and has excellent corrosion resistance in products such as PVC injection molds and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano multilayer composite coatings, and more specifically to an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano multilayer gradient heterogeneous composite coating and a preparation method and application thereof. Background Art

[0002] PVC has been widely used in various covering products due to its excellent flame retardancy and molding properties. However, PVC easily releases highly corrosive HCl gas during plasticization, which seriously corrodes the mold, resulting in a short mold service life, reduced product quality and reduced production efficiency.

[0003] In recent years, PVD nitride coatings have been widely used in hardware processing molds, cutting tools, etc. due to their high hardness, excellent thermal stability and high temperature oxidation resistance. However, single-structure coatings have various defects, resulting in short service life. For example: for columnar crystal structure coatings, the bonding force is high, but the columnar grain boundary is a rapid diffusion channel for the corrosive medium, which can promote the penetration of the corrosive medium into the substrate and accelerate the corrosion and peeling of the coating; nano multilayer structure and nano composite structure have dense organization, but large internal stress, and the coating thickness needs to be reasonably controlled, otherwise it will cause the coating to peel off; high entropy coatings have high hardness and corrosion resistance and high bottom internal stress due to high entropy effect, lattice distortion effect, hysteresis diffusion effect and "cocktail" effect, modulate interfacial stress, improve interfacial bonding behavior, and improve coating bonding. Previous studies have found that single-structure PVD coatings are difficult to meet the strong corrosion requirements of HCl. In addition, when preparing PVD coatings, there are high-density microparticles on the surface of the coating. When the coating is thin, these microparticles run through the entire coating. The interface between the microparticles and the coating substrate is a diffusion channel for the corrosive medium, which is extremely harmful to the corrosion resistance of the coating. Therefore, thin coatings have lower resistance to HCl corrosion. Summary of the invention

[0004] The purpose of the present invention is to provide an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano multilayer gradient heterogeneous composite coating and its preparation method and application, which adopts four coatings of different hardness to overcome the defects of a single coating, and improves the performance of the coating and the substrate bonding strength through the four coating gradient structure designs; by introducing a high-density layered interface, the corrosion medium is inhibited from penetrating into the substrate, and the corrosion resistance of the coating is improved; by regulating the coating thickness, the corrosion resistance of the coating is further improved. This gradient heterogeneous composite coating has high film-substrate bonding strength and corrosion resistance, and has excellent corrosion resistance in products such as PVC injection molds.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is to provide an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano gradient heterogeneous coating, comprising an AlCrN bottom layer, an AlCrN / TiSiN nano multilayer, an AlCrTiSiN high entropy layer and a TiSiN top layer arranged in sequence; wherein the AlCrN / TiSiN nano multilayer is composed of an alternately arranged AlCrN sublayer and a TiSiN sublayer, and is connected to the AlCrN bottom layer and the AlCrTiSiN high entropy layer through the AlCrN sublayer.

[0007] The present invention adopts AlCrN with moderate corrosion resistance and high bonding strength as the bottom layer to improve the film-substrate bonding strength; AlCrN / TiSiN nano multilayer with both hardness and corrosion resistance is used as the second layer, and AlCrN / TiSiN nano multilayer is used to improve the density of the coating and inhibit the growth of penetrating microparticles, greatly reducing the internal growth defects of the coating, thereby improving the corrosion resistance of the coating; AlCrTiSiN high entropy coating with excellent corrosion resistance and toughness is used as the third layer to adjust the interface stress and improve the interlayer bonding strength of the coating. In addition, the thickness of the coating can also be increased; the surface is coated with a TiSiN coating with high hardness to improve the anti-scouring performance of the coating. By regulating the structure of each layer in the gradient heterogeneous composite coating, the coating has high hardness, film-substrate bonding strength and corrosion resistance.

[0008] Furthermore, the AlCrTiSiN high entropy layer and the AlCrN sublayer maintain an epitaxial growth structure, so that the two layers have similar composition, the same structure, and high interlayer bonding strength.

[0009] Furthermore, the AlCrN bottom layer has a thickness of 0.2 to 2.0 μm;

[0010] Furthermore, the AlCrN / TiSiN nano multilayer has a thickness of 2.0 to 8.0 μm, and the single layer thickness of the AlCrN sublayer and the TiSiN sublayer is 5 to 20 nm;

[0011] Furthermore, the AlCrTiSiN high entropy layer has a thickness of 1.0 to 8.0 μm;

[0012] Furthermore, the TiSiN top layer has a thickness of 0.2 to 2.0 μm;

[0013] Furthermore, the total thickness of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano gradient heterogeneous coating is between 3.4 and 20.0 μm.

[0014] Furthermore, the AlCrN bottom layer has a thickness of 0.2 to 2.0 μm, the AlCrN / TiSiN nano multilayer has a thickness of 2.0 to 8.0 μm, the AlCrTiSiN high entropy layer has a thickness of 1.0 to 8.0 μm, and the TiSiN top layer has a thickness of 0.2 to 2.0 μm; the single layer thickness of the AlCrN sublayer and the TiSiN sublayer is 5 to 20 nm.

[0015] The present invention has found through multiple experiments that the coating thickness affects the bonding strength and HCl corrosion resistance of the composite coating. Specifically:

[0016] The AlCrN bottom layer has high affinity and bonding strength with the substrate;

[0017] The TiSiN top layer is a nanocomposite structure with a smooth surface, dense structure and strong corrosion resistance.

[0018] A certain thickness of AlCrN / TiSiN nano multilayer can reduce the internal growth defects (microparticles and holes, etc.) of AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano gradient heterogeneous coating and improve the density of the coating. However, if the AlCrN / TiSiN nano multilayer is too thick, the coating is prone to peeling. Therefore, its thickness needs to be reasonably controlled. In addition, the alternating order of the AlCrN sublayer and the TiSiN sublayer of the AlCrN / TiSiN nano multilayer, and the starting and ending sublayers are AlCrN, which will further improve the corrosion resistance of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN of the present invention.

[0019] The thickness of the AlCrTiSiN high entropy layer affects the corrosion resistance of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano-multilayer gradient heterogeneous composite coating. If the thickness of the AlCrTiSiN high entropy layer is too large (greater than 3μm), it will increase the internal stress of the nano-multilayer gradient heterogeneous composite coating, thereby increasing the brittleness of the coating; while if the thickness is too small (less than 1.0μm), the effect of improving the corrosion resistance of the gradient heterogeneous composite coating is not obvious. That is, the thickness of the AlCrTiSiN high entropy layer is not appropriate, and the corrosion resistance of the coating cannot be effectively improved.

[0020] Furthermore, the AlCrN bottom layer is a columnar crystal structure; the AlCrTiSiN high entropy layer is a single-phase solid solution structure of columnar crystals; and the TiSiN top layer is a nanocomposite structure.

[0021] The second technical solution of the present invention is a method for preparing the above-mentioned nano multi-layer gradient heterogeneous composite coating, comprising the following steps:

[0022] In nitrogen atmosphere, AlCrN bottom layer is physically vapor deposited on the substrate surface using AlCr target;

[0023] In a nitrogen atmosphere, an AlCrN target and a TiSiN target are used to alternately physically vapor deposit AlCrN sublayers and TiSiN sublayers on the surface of an AlCrN bottom layer to obtain an AlCrN / TiSiN nano-multilayer.

[0024] In nitrogen atmosphere, AlCrTiSiN high entropy coating was physically vapor deposited on the surface of AlCrN / TiSiN nano-multilayer using AlCrTiSi target.

[0025] In nitrogen atmosphere, a TiSiN top layer was physically vapor deposited on the surface of the AlCrTiSiN high entropy coating using a TiSi target.

[0026] Furthermore, the substrate is a steel substrate, an aluminum alloy, a titanium alloy or a hard alloy; the substrate is ultrasonically degreased, degreased, cleaned and dried before use.

[0027] Furthermore, an arc ion plating device is used to physically vapor deposit an AlCrN bottom layer on the substrate surface. The specific parameters include: controlling the AlCr target current to 120-200A, the nitrogen flow rate to 300-800sccm, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to 2.0-5.0rpm, and depositing on the substrate surface at 400-550°C for 10-60min.

[0028] Furthermore, AlCrN / TiSiN nano-multilayers were prepared using arc ion plating equipment, and specific parameters included: controlling the current of the AlCr target and the TiSi target to be 120-200A, introducing 500-800sccm of nitrogen, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to be 2.0-5.0rpm, and using the AlCr target and the TiSi target to alternately deposit AlCrN sublayers and TiSiN sublayers on the surface of the AlCrN bottom layer at 400-550°C, the sublayer single layer deposition time is 6-15s, and the total deposition time is 40-150min.

[0029] Furthermore, an AlCrTiSiN high entropy coating was prepared using an arc ion plating device, and specific parameters included: controlling the AlCrTiSi target current to 120-200 A, introducing 500-800 sccm of nitrogen, applying a substrate bias of -40--100 V, controlling the workpiece rotating rack speed in the furnace to 2.0-5.0 rpm, and depositing an AlCrTiSiN high entropy layer on the surface of the AlCrN / TiSiN nano-multilayer at 400-550° C. for a deposition time of 20-60 min.

[0030] Furthermore, an arc ion plating device is used to prepare a TiSiN top layer, and specific parameters include: controlling the TiSi target current to 120 to 200 A, introducing 500 to 800 sccm of nitrogen, applying a substrate bias of -40 to -100 V, controlling the workpiece rotating rack speed in the furnace to 2.0 to 5.0 rpm, and depositing the TiSiN top layer on the surface of the AlCrTiSiN high entropy layer at 400 to 550° C. for a deposition time of 10 to 30 min.

[0031] The third technical solution of the present invention is the application of the above-mentioned nano multi-layer gradient heterogeneous composite coating as injection mold coating and corrosion-resistant parts coating.

[0032] The present invention discloses the following technical effects:

[0033] The present invention adopts AlCrN with moderate corrosion resistance and high bonding strength as the bottom layer, and AlCrN / TiSiN nano multilayer with both hardness and corrosion resistance, and uses AlCrTiSiN high entropy coating with low corrosion resistance internal stress to adjust the interface stress between the nano multilayer and the TiSiN layer, improve the interlayer bonding strength, improve the corrosion resistance of the coating, and effectively increase the thickness of the coating; the hardness and erosion resistance of the coating are improved by the TiSiN coating. Through the above-mentioned multiple structural composite designs, an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating with high bonding strength and excellent corrosion resistance is finally obtained.

[0034] Common methods of physical vapor deposition currently include arc ion plating, evaporation plating, magnetron sputtering and high-power pulse magnetron sputtering. Evaporation plating and magnetron sputtering have low ionization rates, and the bonding between the coating and the substrate is poor; high-power pulse ionization rate is high, but the deposition efficiency is extremely low. In comparison, arc ion plating has high ionization rate and deposition efficiency, and the coating is dense and has high bonding strength. The present invention uses arc ion plating equipment to sequentially deposit an AlCrN bottom layer, an intermediate layer composed of AlCrN / TiSiN and AlCrTiSiN, and a TiSiN surface layer on the surface of the substrate. The nano multilayer gradient composite coating prepared by this method has excellent corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is a schematic diagram of the cross-sectional structure of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating of Example 1.

[0037] Figure 2 This is a physical picture of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating mold prepared using the method of Example 1.

[0038] Figure 3 This is a real picture of the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating mold prepared by the method of Example 1 after serving 600,000 mold cycles.

[0039] Figure 4 This is a physical picture of the AlCrN-AlCrN / TiSiN-AlCrTiSiN gradient heterogeneous composite coating mold prepared by the method of Comparative Example 6.

[0040] Figure 5 This is a real picture of the AlCrN-AlCrN / TiSiN-AlCrTiSiN gradient heterogeneous composite coating mold prepared by the method of Comparative Example 6 after serving 98,000 mold cycles.

[0041] Figure 6 This is the TEM image of the AlCrN / TiSiN nano-multilayer structure prepared in Example 1. DETAILED DESCRIPTION

[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0043] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0047] The target materials used in the following embodiments of the present invention are all commercially available products, specifically: the AlCr target is an Al70Cr30 target (70 at.% Al, 30 at.% Cr); the TiSi target is a Ti85Si15 target; and the AlCrTiSi target is an Al35Cr20Ti30Si15 target.

[0048] Example 1

[0049] This embodiment provides an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating, including an AlCrN layer, an AlCrN / TiSiN layer, an AlCrTiSiN layer and a TiSiN layer connected in sequence, wherein the AlCrN layer is the bottom layer, and the bottom layer is connected to S136 mold steel (commercially available).

[0050] A method for preparing an AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN gradient heterogeneous composite coating comprises the following steps:

[0051] S1: ultrasonically degreasing, degreasing, cleaning and drying the substrate;

[0052] S2: Using arc ion plating equipment, controlling the AlCr target current to 160A, the nitrogen flow rate to 500sccm, applying a substrate bias of -40V, controlling the workpiece rotating rack speed in the furnace to 3.5rpm, and depositing on the substrate surface at 450℃ for 20min to obtain an AlCrN bottom layer with a thickness of 0.4μm;

[0053] S3: Control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit time 120min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit AlCrN sublayer and TiSiN sublayer on the surface of AlCrN bottom layer at 450℃ to form AlCrN / TiSiN layer with a thickness of 6μm and a single sublayer thickness of 8nm; specifically, first use AlCr target to deposit AlCrN sublayer with a thickness of 8nm, then use TiSi target to deposit TiSiN sublayer with a thickness of 8nm, alternate deposition, and finally use AlCr target to deposit AlCrN sublayer with a thickness of 8nm. So far, AlCrN-AlCrN / TiSiN layer is obtained;

[0054] S4: Control the AlCrTiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 60min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit an AlCrTiSiN high entropy layer on the AlCrN-AlCrN / TiSiN layer at 450℃ with a thickness of 3.0μm. Thus, the AlCrN-AlCrN / TiSiN-AlCrTiSiN layer is obtained;

[0055] S5: Control the TiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 20min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit a TiSiN high entropy layer on the AlCrN-AlCrN / TiSiN-AlCrTiSiN layer at 450℃ with a thickness of 1.0μm. Thus, the AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN heterogeneous composite coating is obtained with a thickness of 10.4μm and a structure as shown below: Figure 1 shown.

[0056] Embodiments 2 to 6

[0057] Examples 2 to 6 provide different AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano multilayer gradient composite coatings, each of which includes AlCrN, AlCrN / TiSiN, AlCrTiSiN and TiSiN layers connected in sequence. Among them, the AlCrN layer is the bottom layer, and the bottom layer is connected to the substrate. The difference from Example 1 is that the parameters when preparing each layer are different. The specific parameters of Examples 2-6 are shown in Tables 1-5.

[0058] Table 1 Experimental parameters for preparing AlCrN bottom layer

[0059]

[0060] Table 2 Experimental parameters for preparing AlCrN / TiSiN nano-multilayers in Examples 2 to 6

[0061]

[0062]

[0063] Table 3 Experimental parameters for preparing AlCrTiSiN high entropy layer in Examples 2 to 6

[0064]

[0065] Table 4 Experimental parameters for preparing TiSiN top layer in Examples 2 to 6

[0066]

[0067] Table 5 Coating thickness of AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN nano multilayer gradient composite coating of Examples 2 to 6

[0068]

[0069] Example 7

[0070] Same as embodiment 1, the only difference is that S2 and S3 are swapped.

[0071] Example 8

[0072] The same as embodiment 1, the only difference is that S2 and S4 are swapped.

[0073] Example 9

[0074] The same as embodiment 1, the only difference is that S3 and S4 are swapped.

[0075] Example 10

[0076] The same as embodiment 1, the only difference is that S3 and S5 are swapped.

[0077] Embodiment 11

[0078] The same as embodiment 1, the only difference is that S4 and S5 are swapped.

[0079] Example 12

[0080] Same as embodiment 1, the only difference is that S2 and S5 are swapped.

[0081] Comparative Example 1

[0082] This comparative example provides an AlCrN layer, and the preparation method thereof comprises the following steps:

[0083] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0084] S2: Using arc ion plating equipment, the AlCr target current was controlled to be 160A, nitrogen was introduced at 500sccm, a substrate bias of -40V was applied, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and deposition was performed on the substrate surface at 450°C for 20min to obtain an AlCrN layer with a thickness of 0.4μm.

[0085] Comparative Example 2

[0086] This comparative example provides an AlCrN / TiSiN nano-multilayer, and its preparation method comprises the following steps:

[0087] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0088] S2: Using arc ion plating equipment, control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit on the substrate surface at 450℃ for 2h to obtain AlCrN / TiSiN nano multilayer with a thickness of 6.0μm. Specifically, first use AlCr target to deposit an AlCrN sublayer with a thickness of 8nm, then use TiSi target to deposit a TiSiN sublayer with a thickness of 2.5nm, alternately deposit, and finally use AlCr target to deposit an AlCrN sublayer with a thickness of 8nm.

[0089] Comparative Example 3

[0090] This comparative example provides an AlCrTiSiN layer, and the preparation method thereof comprises the following steps:

[0091] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0092] S2: Using arc ion plating equipment, the AlCrTiSi target current was controlled to be 160A, 600sccm of nitrogen was introduced, a substrate bias of -60V was applied, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and deposition was performed on the substrate surface at 450°C for 60min to obtain an AlCrTiSiN layer with a thickness of 3.0μm.

[0093] Comparative Example 4

[0094] This comparative example provides a TiSiN layer, and the preparation method thereof comprises the following steps:

[0095] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0096] S2: Using arc ion plating equipment, the TiSi target current was controlled to be 145A, 500sccm of nitrogen was introduced, a substrate bias of -60V was applied, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and AlCrTiSiN layer was deposited on the substrate surface at 450°C for 30min to obtain a layer with a thickness of 1.0μm.

[0097] Comparative Example 5

[0098] This comparative example provides an AlCrN-AlCrN / TiSiN layer, comprising an AlCrN bottom layer and an AlCrN / TiSiN nano-multilayer connected in sequence, and a preparation method thereof comprises the following steps:

[0099] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0100] S2: Using arc ion plating equipment, the AlCr target current was controlled to be 160A, nitrogen was introduced at 500sccm, the substrate bias was applied at -40V, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and the AlCrN layer was deposited on the surface of S136 mold steel at 420℃ for 20min, and the AlCrN layer was obtained with a thickness of 0.4μm;

[0101] S3: Control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit on AlCrN layer at 450℃ for 120min to obtain AlCrN / TiSiN nano-multilayer with a thickness of 6μm; thus, AlCrN-AlCrN / TiSiN layer with a thickness of 6.4μm is obtained. Specifically, first use AlCr target to deposit AlCrN sublayer with a thickness of 8nm, then use TiSi target to deposit TiSiN sublayer with a thickness of 2.5nm, alternately deposit, and finally use AlCr target to deposit AlCrN sublayer with a thickness of 8nm. Thus, AlCrN-AlCrN / TiSiN layer is obtained.

[0102] Comparative Example 6

[0103] This comparative example provides an AlCrN-AlCrN / TiSiN-AlCrTiSiN layer, comprising an AlCrN bottom layer, an AlCrN / TiSiN nano-multilayer and an AlCrTiSiN high entropy layer connected in sequence, and a preparation method thereof comprises the following steps:

[0104] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0105] S2: Using arc ion plating equipment, the AlCr target current was controlled to be 160A, nitrogen was introduced at 500sccm, the substrate bias was applied at -40V, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and the AlCrN layer was deposited on the surface of S136 mold steel at 420℃ for 20min, and the AlCrN layer was obtained with a thickness of 0.4μm;

[0106] S3: Control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit on AlCrN layer at 450℃ for 120min to obtain AlCrN / TiSiN nano-multilayer with a thickness of 6μm; thus, AlCrN-AlCrN / TiSiN layer with a thickness of 6.4μm is obtained. Specifically, first use AlCr target to deposit AlCrN sublayer with a thickness of 8nm, and then use TiSi target to deposit TiSiN sublayer with a thickness of 2.5nm, alternately deposit, and finally use AlCr target to deposit AlCrN sublayer with a thickness of 8nm. Thus, AlCrN-AlCrN / TiSiN layer is obtained;

[0107] S4: Control the AlCrTiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 60min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit an AlCrTiSiN high entropy layer on the AlCrN-AlCrN / TiSiN layer at 450℃ with a thickness of 3.0μm. Thus, the AlCrN-AlCrN / TiSiN-AlCrTiSiN layer is obtained. Its total thickness is 9.4μm.

[0108] Comparative Example 7

[0109] This comparative example provides an AlCrN-AlCrN / TiSiN-TiSiN layer, comprising an AlCrN bottom layer, an AlCrN / TiSiN nano-multilayer and a TiSiN layer connected in sequence, and a preparation method thereof comprises the following steps:

[0110] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0111] S2: Using arc ion plating equipment, the AlCr target current was controlled to be 160A, nitrogen was introduced at 500sccm, the substrate bias was applied at -40V, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, and the AlCrN layer was deposited on the surface of S136 mold steel at 420℃ for 20min, and the AlCrN layer was obtained with a thickness of 0.4μm;

[0112] S3: Control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit on AlCrN layer at 450℃ for 120min to obtain AlCrN / TiSiN nano multilayer with a thickness of 6.0μm; specifically, first use AlCr target to deposit AlCrN sublayer with a thickness of 8nm, then use TiSi target to deposit TiSiN sublayer with a thickness of 2.5nm, alternately deposit, and finally use AlCr target to deposit AlCrN sublayer with a thickness of 8nm. So far, AlCrN-AlCrN / TiSiN layer is obtained;

[0113] S4: Control the TiSi target current to 160A, introduce 500sccm of nitrogen, apply substrate bias voltage -60V, deposit time 30min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit a TiSiN layer on the AlCrN-AlCrN / TiSiN layer at 450℃ with a thickness of 1.5μm. Thus, the AlCrN-AlCrN / TiSiN-TiSiN layer is obtained. Its total thickness is 7.9μm.

[0114] Comparative Example 8

[0115] This comparative example provides an AlCrN / TiSiN-AlCrTiSiN-TiSiN layer, comprising an AlCrN / TiSiN nano-multilayer, an AlCrTiSiN high entropy layer and a TiSiN layer connected in sequence, and a preparation method thereof comprises the following steps:

[0116] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0117] S2: Control the current of AlCr target and TiSi target to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, control the workpiece rotating rack speed in the furnace to 3.5rpm, and use AlCr target and TiSi target to alternately deposit on the substrate at 450℃ for 120min to obtain AlCrN / TiSiN nano-multilayer with a thickness of 6.0μm. Specifically, first use AlCr target to deposit an AlCrN sublayer with a thickness of 8nm, then use TiSi target to deposit a TiSiN sublayer with a thickness of 2.5nm, alternately deposit, and use AlCr target to deposit an AlCrN sublayer with a thickness of 8nm for the last time;

[0118] S3: Control the AlCrTiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 30min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit an AlCrTiSiN layer on the AlCrN / TiSiN layer at 450℃ with a thickness of 1.5μm. Thus, an AlCrN / TiSiN-AlCrTiSiN layer is obtained with a total thickness of 7.5μm;

[0119] S4: Control the TiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 20min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit a TiSiN layer on the AlCrN / TiSiN-AlCrTiSiN layer at 450°C with a thickness of 1.0μm. Thus, an AlCrN / TiSiN-AlCrTiSiN-TiSiN heterogeneous composite coating with a thickness of 8.5μm is obtained.

[0120] Comparative Example 9

[0121] This comparative example provides an AlCrN-AlCrTiSiN-TiSiN layer, comprising an AlCrN layer, an AlCrTiSiN high entropy layer and a TiSiN layer connected in sequence, and a preparation method thereof comprises the following steps:

[0122] S1: Ultrasonic degreasing, degreasing, cleaning and drying of S136 mold steel;

[0123] S2: The AlCr target current was controlled to be 160A, nitrogen was introduced at 500sccm, a substrate bias voltage of -40V was applied, the workpiece rotating rack speed in the furnace was controlled to be 3.5rpm, AlCr was deposited at 450°C for 20min, and an AlCrN layer with a thickness of 0.4μm was obtained;

[0124] S3: Control the AlCrTiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit time 30min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit an AlCrTiSiN layer on the AlCrN layer at 450℃ with a thickness of 1.5μm. Thus, an AlCrN-AlCrTiSiN layer is obtained with a total thickness of 1.35μm;

[0125] S4: Control the TiSi target current to 160A, introduce nitrogen gas at 600sccm, apply substrate bias voltage -60V, deposit for 20min, control the workpiece rotating rack speed in the furnace to 3.5rpm, and deposit a TiSiN layer on the AlCrN-AlCrTiSiN layer at 450°C with a thickness of 1.0μm. Thus, an AlCrN-AlCrTiSiN-TiSiN heterogeneous composite coating with a thickness of 2.9μm is obtained.

[0126] Test example

[0127] The following methods were used to test the performance of the coatings in the examples and comparative examples. The results are shown in Tables 6-7:

[0128] 1. Use a multifunctional scratch tester to test the bonding strength between the coating and the substrate, with a test load of 0 to 120N;

[0129] 2. The corrosion potential of each coating in 10 vol.% HCl aqueous solution was measured using an electrochemical workstation;

[0130] 3. The coated molds of Example 1 and Comparative Example 6 were used for ABS+40% PVC mixed injection molding. When pitting visible to the naked eye appeared on the surface of the injection molded product, the coated mold was determined to be ineffective.

[0131] Table 6 Performance results of composite coatings of Examples 1 to 12

[0132]

[0133]

[0134] Examples 7-12 have the same layer thickness as Example 1, but in a different order.

[0135] Table 7 Performance test results of coatings of Example 1 and Comparative Examples 1 to 9

[0136]

[0137] It can be seen from Table 6 and Table 7 that the coating of Examples 1 to 6 of the present invention has a bonding force with the substrate in the range of 76 to 120 N, and a corrosion potential in the range of -0.02 to 0.18 V, while Comparative Examples 1 to 9, compared with Example 1, have not achieved a joint improvement in substrate bonding force and corrosion resistance. Compared with Examples 7-12, under the same preparation parameters, only the coating sequence has changed in Example 1, which makes the bonding force and corrosion resistance of the product of Example 1 better. Combined with the experimental results of omitting a certain coating in Comparative Examples 6-9, it is shown that the structure and composition of the coating of the present invention have a significant impact on the product performance; in addition, when a single AlCrN / TiSiN coating, AlCrTiSiN coating or TiSiN coating is used, although the coating has better bonding force, the corrosion resistance is not good; therefore, the coating sequence of AlCrN-AlCrN / TiSiN-AlCrTiSiN-TiSiN of the present invention is the optimal combination. The present invention can effectively improve the corrosion resistance and bonding strength of the coating by matching four different compositions of the AlCrN bottom layer, the AlCrN / TiSiN nano multilayer, the AlCrTiSiN high entropy layer and the TiSiN nano composite layer structure.

[0138] When ABS+40%PVC mixed injection molding is processed, the service life of the mold in Example 1 reaches 600,000 times ( Figure 3 ), the coating on the mold surface still exists, while the mold of comparative example 6 has been in service for less than 100,000 times, the coating on the mold surface has peeled off, and there are high-density pitting defects on the surface of the product, and the coated mold has failed ( Figure 5 ).

[0139] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A nano multilayer gradient heterogeneous composite coating, characterized in that: It includes an AlCrN bottom layer, an AlCrN / TiSiN nano-multilayer, an AlCrTiSiN high entropy layer and a TiSiN top layer arranged in sequence; wherein the AlCrN / TiSiN nano-multilayer is composed of an AlCrN sublayer and a TiSiN sublayer arranged alternately, and is connected to the AlCrN bottom layer and the AlCrTiSiN high entropy layer through the AlCrN sublayer.

2. The nano multi-layer gradient heterogeneous composite coating according to claim 1, characterized in that: The thickness of the AlCrN bottom layer is 0.2-2.0 μm; the thickness of the AlCrN / TiSiN nano multilayer is 2.0-8.0 μm; the thickness of the AlCrTiSiN high entropy layer is 1.0-8.0 μm; the thickness of the TiSiN top layer is 0.2-2.0 μm; the single layer thickness of the AlCrN sublayer and the TiSiN sublayer is 5-20 nm.

3. The nano multi-layer gradient heterogeneous composite coating according to claim 1, characterized in that: The AlCrN bottom layer is a columnar crystal structure; the AlCrTiSiN high entropy layer is a single-phase solid solution structure of columnar crystals; and the TiSiN top layer is a nanocomposite structure.

4. A method for preparing a nano multilayer gradient heterogeneous composite coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: In nitrogen atmosphere, AlCrN bottom layer is physically vapor deposited on the substrate surface using AlCr target; In a nitrogen atmosphere, an AlCrN target and a TiSiN target are used to alternately physically vapor deposit AlCrN sublayers and TiSiN sublayers on the surface of an AlCrN bottom layer to obtain an AlCrN / TiSiN nano-multilayer. In nitrogen atmosphere, AlCrTiSiN high entropy coating was physically vapor deposited on the surface of AlCrN / TiSiN nano-multilayer using AlCrTiSi target. In nitrogen atmosphere, a TiSiN top layer was physically vapor deposited on the surface of the AlCrTiSiN high entropy coating using a TiSi target.

5. The method for preparing the nano multi-layer gradient heterogeneous composite coating according to claim 4, characterized in that: The substrate is a steel substrate, an aluminum alloy, a titanium alloy or a hard alloy; the substrate is ultrasonically degreased, degreased, cleaned and dried before use.

6. The method for preparing the nano multi-layer gradient heterogeneous composite coating according to claim 4, characterized in that: The AlCrN bottom layer is physically vapor deposited on the substrate surface using arc ion plating equipment. The specific parameters include: controlling the AlCr target current to 120-200A, the nitrogen flow rate to 300-800sccm, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to 2.0-5.0rpm, and depositing on the substrate surface at 400-550°C for 10-60min.

7. The method for preparing a nano multilayer gradient heterogeneous composite coating according to claim 4, characterized in that: AlCrN / TiSiN nano-multilayers were prepared using arc ion plating equipment, and the specific parameters included: controlling the current of the AlCr target and the TiSi target to be 120-200A, introducing 500-800sccm of nitrogen, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to be 2.0-5.0rpm, and alternately depositing AlCrN sublayers and TiSiN sublayers on the surface of the AlCrN bottom layer using the AlCr target and the TiSi target at 400-550°C, the sublayer single layer deposition time is 6-15s, and the total deposition time is 40-150min.

8. The method for preparing a nano multi-layer gradient heterogeneous composite coating according to claim 4, characterized in that: The AlCrTiSiN high entropy coating was prepared using an arc ion plating device. The specific parameters included: controlling the AlCrTiSi target current to 120-200A, introducing 500-800sccm of nitrogen, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to 2.0-5.0rpm, and depositing an AlCrTiSiN high entropy layer on the surface of the AlCrN / TiSiN nano-multilayer at 400-550°C for 20-60min.

9. The method for preparing a nano multilayer gradient heterogeneous composite coating according to claim 4, characterized in that: The TiSiN top layer is prepared by arc ion plating equipment. The specific parameters include: controlling the TiSi target current to 120-200A, introducing 500-800sccm of nitrogen, applying a substrate bias of -40--100V, controlling the workpiece rotating rack speed in the furnace to 2.0-5.0rpm, and depositing the TiSiN top layer on the surface of the AlCrTiSiN high entropy layer at 400-550°C for 10-30min.

10. Use of the nano multi-layer gradient heterogeneous composite coating according to any one of claims 1 to 3 as an injection mold coating or a corrosion-resistant parts coating.

Citation Information

Patent Citations

  • AlTiN-AlCrN super hard nano multilayer composite coating hob and preparation method thereof

    CN102922052A

  • Superhard strong toughness and high-entropy alloy nitride nano-composite coating carbide blade and preparation method thereof

    CN108642449A

  • Single-phase solid solution structure AlCrTiSiN high-entropy alloy nitride coating and preparation method and application thereof

    CN109881148A

  • High red hardness AlCrN / AlTiN nano multilayer coating and preparation method thereof

    CN113930722A

  • Preparation method of AlCrTiSiN nano-composite coating plated alloy saw blade

    CN115354282A