High-efficiency deep ultraviolet light-emitting diode with stepped composition YAlN / AlGaN superlattice p-type layer and preparation method thereof
By using the step component YAlN/AlGaN superlattice p-type layer in the deep ultraviolet light emitting diode, the problems of low Mg ionization rate and insufficient hole concentration in the high AlGaN p-type layer are solved, and the luminous efficiency and Crystal mass.
Patent Information
- Application Number
- CN202210713333.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-06-22
AI Technical Summary
In the existing deep ultraviolet light emitting diodes, the AlGaN p-type layer with high Al component leads to low ionization rate of Mg and insufficient hole concentration, affecting the luminescence efficiency of the device, and it is difficult to contact the ohmic with the metal electrode and lattice mismatch. Causes poor crystal quality.
The superlattice p-type layer of the ladder component YAlN/AlGaN superlattice p-type layer was used to grow the superlattice structure of the third-step ladder component through the MOCVD process, and the polarization effect of YAlN was used to increase the ionization rate of Mg, and the epitaxiality was reduced by decreasing Al component. The stress of the layer improves the crystal quality.
It effectively improves carrier concentration, reduces electron leakage, improves luminous power and efficiency, and improves the crystal epitaxial quality of the device.
Smart Images

Figure CN115064620B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microelectronic technology, and in particular relates to a high-efficiency deep ultraviolet light-emitting diode, which can be used to manufacture high-efficiency ultraviolet and deep ultraviolet light-emitting devices. Technical Background
[0002] AlGaN ternary alloy can adjust the band gap between 3.43eV and 6.11eV, and is suitable for the manufacture of optical devices in the wavelength range of 200nm-365nm. In this wavelength range, applications include sterilization, UV curing and printing, phototherapy and medical applications, photocatalyst deodorization and material sensing. So far, these applications mainly use traditional mercury lamps. Compared with mercury lamps, UV light-emitting diodes have many advantages such as low cost, small size, long life, good stability, high safety and environmental protection. AlGaN-based UV light-emitting diodes are very likely to become a new type of UV light source to replace mercury lamps in the future.
[0003] P-type doping is an important factor affecting the efficiency of light-emitting diodes, but good p-type doping has always been a problem. Mg is the most commonly used p-type dopant in light-emitting diodes. The activation energy of Mg as an acceptor dopant in GaN is 200 meV. As the band gap increases, the activation energy in AlN reaches 630 meV. The high activation energy leads to a very low ionization rate. In the ultraviolet and deep ultraviolet spectral regions, as the Al component of AlGaN increases, the ionization rate of Mg decreases significantly. At present, it is very difficult to achieve efficient ionization of Mg in AlGaN. The hole concentration in current p-type AlGaN is generally low, generally around 10 17 cm -3 The lower hole concentration inhibits the development of high-efficiency UV LEDs. Therefore, in order to improve the efficiency of UV LEDs, it is necessary to increase the hole concentration.
[0004] At present, conventional deep ultraviolet light-emitting diodes include a substrate, a nucleation layer, a buffer layer, an n-type layer, a multi-quantum well layer, an electron blocking layer, a p-type layer, and an ohmic contact layer, such as Figure 1 As shown, the p-type layer mainly uses uniformly doped AlGaN material. This device has the following three disadvantages:
[0005] First, for deep ultraviolet LEDs, the material used for the p-type layer is AlGaN with a high Al component. The activation energy of Mg is very high and the ionization efficiency is low, which leads to a very low hole activation efficiency, affecting the luminous efficiency of the LED.
[0006] Second, the low hole concentration makes the electron-hole balance more unbalanced, further aggravating electron leakage and reducing device efficiency.
[0007] Third, for deep ultraviolet LEDs, the material used for the p-type layer is AlGaN with a high Al component. However, it is very difficult for AlGaN with a high Al component to form an ohmic contact with the metal electrode. The GaN layer is often used as the ohmic contact layer. However, there is a large lattice mismatch between AlGaN and GaN, and there is a large stress between the layers. The crystal quality is poor, and the epitaxial process is difficult. Summary of the invention
[0008] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and propose a high-efficiency deep ultraviolet light-emitting diode with a stepped-composition YAlN / AlGaN superlattice p-type layer and a manufacturing method, so as to utilize the polarization electric field of the superlattice to effectively increase the ionization rate of Mg doping, increase the carrier concentration, reduce electron leakage, and effectively improve the device's luminous power and efficiency, and reduce the stress in the epitaxial layer by adopting a stepped-composition p-type layer to improve the crystal epitaxial quality.
[0009] The technical solution for achieving the purpose of the present invention is as follows:
[0010] 1. A high-efficiency deep ultraviolet light-emitting diode with a stepped composition YAlN / AlGaN superlattice p-type layer, which comprises from bottom to top: a substrate, a nucleation layer, a buffer layer, an n-type layer, a multi-quantum well layer, an electron blocking layer, a p-type layer, and an ohmic contact layer, characterized in that:
[0011] The p-type layer adopts a three-step stepped component YAlN / AlGaN superlattice, and the parameters of each step are as follows:
[0012] The number of first-order superlattice periods is 7-10, the Al component of YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of AlGaN material in each period ranges from 0.5-0.8, the thickness is 1nm-4nm;
[0013] The number of periods of the second-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.3-0.5, the thickness is 1nm-4nm;
[0014] The number of periods of the third-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.1-0.3, the thickness is 1nm-4nm;
[0015] The Al component of the AlGaN material in the three stages decreases gradually, forming a YAlN / AlGaN superlattice p-type layer with a stepped composition, so as to effectively improve the luminous efficiency of the device.
[0016] Furthermore, the multi-quantum well layer includes five periods of quantum wells and quantum barriers, each period of quantum wells uses AlGaN material with a thickness of 1.3nm-3nm and an Al component of 0.4-0.79, and each period of quantum barriers uses AlGaN material with a thickness of 7nm-12nm and an Al component of 0.5-0.87.
[0017] Furthermore, the substrate is made of c-plane sapphire material.
[0018] Furthermore, the nucleation layer is made of high-temperature AlN material with a thickness of 15nm-35nm.
[0019] Furthermore, the buffer layer is made of AlN material with a thickness of 1 μm-2 μm.
[0020] Furthermore, the ohmic contact layer is made of GaN material with a thickness of 10nm-20nm.
[0021] Furthermore, the n-type layer is made of AlGaN material with a thickness of 1.5 μm-2.5 μm and an Al component of 0.6-0.9.
[0022] Furthermore, the electron blocking layer is made of AlGaN material with a thickness of 20nm-30nm and an Al component of 0.65-0.98.
[0023] 2. A method for manufacturing a high-efficiency deep ultraviolet light-emitting diode with a stepped composition YAlN / AlGaN superlattice p-type layer, characterized in that it comprises the following steps:
[0024] 1) Pre-treatment of cleaning and nitridation of the substrate;
[0025] 2) growing a 15nm-35nm nucleation layer on the pretreated substrate using a MOCVD process;
[0026] 3) On the nucleation layer, a buffer layer of 1 μm-2 μm is grown using a MOCVD process;
[0027] 4) On the buffer layer, a 1.5 μm-2.5 μm n-type layer is grown using a MOCVD process;
[0028] 5) On the n-type layer, a multi-quantum well layer including five periods of quantum wells and quantum barriers is grown by MOCVD process, wherein the thickness of the quantum well of each period is 1.3nm-3nm, and the thickness of the quantum barrier of each period is 7nm-12nm;
[0029] 6) On the multi-quantum well layer, an electron blocking layer with a thickness of 20nm-30nm is grown by MOCVD process;
[0030] 7) On the electron blocking layer, a three-step stepped YAlN / AlGaN superlattice p-type layer with decreasing Al composition is grown using the MOCVD process:
[0031] 7a) growing a first-order superlattice with a period of 7-10 on the electron blocking layer by MOCVD process, wherein the thickness of the YAlN material in each period of the first-order superlattice is 3nm-7nm, the thickness of the AlGaN material in each period is 1nm-4nm, and the Al component range is 0.5-0.8;
[0032] 7b) growing a second-order superlattice with a period of 7-10 on the first-order superlattice by MOCVD process, wherein the thickness of the YAlN material of each period of the second-order superlattice is 3nm-7nm, the thickness of the AlGaN material of each period is 1nm-4nm, and the Al composition ranges from 0.3 to 0.5;
[0033] 7c) growing a third-order superlattice with a period of 7-10 on the second-order superlattice by MOCVD process, wherein the thickness of the YAlN material of each period of the third-order superlattice is 3nm-7nm, the thickness of the AlGaN material of each period is 1nm-4nm, and the Al composition ranges from 0.1 to 0.3;
[0034] 8) On the p-type layer, an ohmic contact layer with a thickness of 10 nm to 20 nm is grown using a MOCVD process;
[0035] 9) The ohmic contact layer is etched by dry etching, the etching depth is from the surface to the middle of the n-type layer, and the etching shape is a sector with a central angle of 90°;
[0036] 10) Using a metal sputtering method, metal is deposited on the unetched ohmic contact layer to form a p-electrode, and using a metal sputtering method, metal is deposited on the etched n-type layer to form an n-electrode, thereby completing the production of the LED.
[0037] Compared with the prior art, the present invention has the following advantages:
[0038] 1. The present invention adopts YAlN / AlGaN superlattice as the p-type layer. Since YAlN is a transition metal nitride with a strong polarization effect, it can effectively increase the ionization rate of Mg by using a strong polarization electric field, increase the carrier concentration, improve electron leakage, and improve the luminous power and efficiency of the device.
[0039] 2. The YAlN / AlGaN superlattice of the present invention adopts a stepped composition with decreasing Al composition, which effectively reduces the stress in the epitaxial layer and improves the quality of crystal epitaxy. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1It is the overall structure diagram of the high-efficiency deep ultraviolet light-emitting diode of the present invention;
[0041] Figure 2 yes Figure 1 Schematic diagram of the structure of the p-type layer of the medium-step composition YAlN / AlGaN superlattice;
[0042] Figure 3 The invention is made Figure 1 Schematic diagram of the realization process of high-efficiency deep ultraviolet light-emitting diodes. DETAILED DESCRIPTION
[0043] The embodiments of the present invention are further described in detail below with reference to the accompanying drawings.
[0044] Reference Figure 1 The deep ultraviolet light-emitting diode of the present invention comprises a substrate 1, a nucleation layer 2, a buffer layer 3, an n-type layer 4, a multi-quantum well layer 5, an electron blocking layer 6, a YAlN / AlGaN superlattice p-type layer 7, and an ohmic contact layer 8. Wherein:
[0045] The substrate 1 is made of c-plane sapphire material;
[0046] The nucleation layer 2 is made of high temperature AlN material with a thickness of 15nm-35nm and is located on the substrate;
[0047] The buffer layer 3 is made of AlN material and has a thickness of 1 μm-2 μm, and is located on the nucleation layer;
[0048] The n-type layer 4 is made of AlGaN material, with an Al composition range of 0.6-0.9 and a thickness of 1.5 μm-2.5 μm, and is located on the buffer layer;
[0049] The multi-quantum well layer 5 includes five periods of quantum wells and quantum barriers, each period of quantum wells is made of AlGaN material, the Al component range is 0.4-0.79, and the thickness is 1.3nm-3nm; each period of quantum barriers is made of AlGaN material, the Al component range is 0.5-0.87, and the thickness is 7nm-12nm; the total thickness of all periodic quantum wells and quantum barriers is 41.5nm-75nm, which is located on the n-type layer;
[0050] The electron blocking layer 6 is made of AlGaN material, with an Al composition range of 0.65-0.98 and a thickness of 20nm-30nm, and is located on the multi-quantum well layer;
[0051] Reference Figure 2 The YAlN / AlGaN superlattice p-type layer 7 adopts a three-step stepped component YAlN / AlGaN superlattice, and the parameters of each step are as follows:
[0052] The number of first-order superlattice periods is 7-10, the Al component of YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of AlGaN material in each period ranges from 0.5-0.8, the thickness is 1nm-4nm;
[0053] The number of periods of the second-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.3-0.5, the thickness is 1nm-4nm;
[0054] The number of periods of the third-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.1-0.3, the thickness is 1nm-4nm;
[0055] The Al component of the AlGaN material in the three steps decreases gradually, forming a YAlN / AlGaN superlattice p-type layer with a stepped composition, which is located above the electron blocking layer;
[0056] The ohmic contact layer 8 is made of GaN material and has a thickness of 10nm-20nm. It is located on the p-type layer.
[0057] Reference Figure 3 The present invention provides three embodiments for preparing high-efficiency deep ultraviolet light-emitting diodes with a stepped composition YAlN / AlGaN superlattice p-type layer.
[0058] Example 1: Prepare a deep ultraviolet light emitting diode with a light emission wavelength of 280nm.
[0059] Step 1: pre-treating the substrate.
[0060] 1.1) Clean the c-plane sapphire substrate and place the cleaned substrate in the MOCVD reaction chamber. Reduce the vacuum degree of the reaction chamber to 2×10 -2 Torr, hydrogen is introduced into the reaction chamber, and when the pressure in the MOCVD reaction chamber reaches 30 Torr, the temperature of the substrate is heated to 1050°C and maintained for 5 minutes to complete the heat treatment of the substrate.
[0061] 1.2) The heat-treated substrate was placed in a reaction chamber at a temperature of 1200° C., and ammonia gas was introduced at a flow rate of 3000 sccm for nitridation for 5 minutes to complete the pretreatment of the substrate.
[0062] Step 2: epitaxial nucleation layer, such as Figure 3 (a) shown.
[0063] The temperature of the reaction chamber was raised to 1250° C., the pressure of the reaction chamber was maintained at 30 Torr, and a nitrogen source with a flow rate of 2000 sccm and an aluminum source with a flow rate of 20 sccm were introduced at the same time. A high-temperature AlN nucleation layer 2 with a thickness of 35 nm was grown on the c-plane sapphire substrate using the MOCVD method.
[0064] Step 3, epitaxial buffer layer, such as Figure 3 (b) as shown.
[0065] The temperature of the reaction chamber was maintained at 1250° C., the pressure of the reaction chamber was maintained at 30 Torr, and a nitrogen source with a flow rate of 2000 sccm and an aluminum source with a flow rate of 20 sccm were introduced at the same time. An AlN buffer layer 3 with a thickness of 1 μm was grown on the nucleation layer by MOCVD method.
[0066] Step 4: epitaxially grow the n-type layer, such as Figure 3 (c) as shown.
[0067] The temperature of the reaction chamber was lowered to 1150°C, the pressure of the reaction chamber was lowered to 20 Torr, and a nitrogen source with a flow rate of 2500 sccm, a gallium source with a flow rate of 60 sccm, an aluminum source with a flow rate of 150 sccm, and a silicon source with a flow rate of 40 sccm were introduced at the same time. The MOCVD method was used to grow an n-type Al with a thickness of 2.5 μm on the buffer layer. 0.6 Ga 0.4 N-layer 4.
[0068] Step 5, epitaxial multi-quantum well layer, such as Figure 3 (d) as shown.
[0069] The reaction chamber temperature was maintained at 1150°C, the reaction chamber pressure was maintained at 20 Torr, and a nitrogen source with a flow rate of 2500 sccm was introduced. Five cycles of Al were grown on the n-type layer using the MOCVD method. 0.4 Ga 0.6 N / A 0.5 Ga 0.5 N multi-quantum well layer 5:
[0070] 5.1) A gallium source with a flow rate of 120 sccm and an aluminum source with a flow rate of 150 sccm are introduced to grow an Al layer with a thickness of 12 nm on the n-type layer. 0.5 Ga 0.5 N quantum barrier layers;
[0071] 5.2) A gallium source with a flow rate of 100 sccm and an aluminum source with a flow rate of 120 sccm are introduced to grow a 3 nm thick Al layer on the quantum barrier layer. 0.4 Ga 0.6 N quantum well layer;
[0072] 5.3) Repeat 5.1) and 5.2) for five cycles of alternating growth to obtain a multi-quantum well layer.
[0073] Step 6: epitaxial electron blocking layer, such as Figure 3 (e) as shown.
[0074] The temperature of the reaction chamber was raised to 1200°C, the pressure of the reaction chamber was raised to 30 Torr, and a nitrogen source with a flow rate of 1800 sccm, a gallium source with a flow rate of 50 sccm, and an aluminum source with a flow rate of 120 sccm were introduced at the same time. Al with a thickness of 30 nm was grown on the multi-quantum well layer using the MOCVD method. 0.65 Ga 0.35 N electron blocking layer 6.
[0075] Step 7, epitaxial p-type layer, such as Figure 3 (f) as shown.
[0076] The temperature of the reaction chamber was lowered to 1050°C, the pressure of the reaction chamber was maintained at 30 Torr, a nitrogen source with a flow rate of 2500 sccm and a magnesium source with a flow rate of 200 sccm were introduced at the same time, and then a three-step ladder superlattice was grown according to the following process conditions:
[0077] 7.1) Using MOCVD method to grow the first-order superlattice on the electron blocking layer:
[0078] 7.1.1) A yttrium source with a flow rate of 50 sccm and an aluminum source with a flow rate of 320 sccm are introduced into the reaction chamber to grow a 6 nm thick Y layer on the electron blocking layer. 0.2 Al 0.8 N layers;
[0079] 7.1.2) A gallium source with a flow rate of 150 sccm and an aluminum source with a flow rate of 120 sccm are introduced into the reaction chamber. 0.2 Al 0.8 A 3nm thick Al layer is grown on the N layer. 0.5 Ga 0.5 N layers;
[0080] 7.1.3) Repeat 7.1.1) and 7.1.2) for 10 cycles to obtain the first-order superlattice;
[0081] 7.2) Using MOCVD method to grow the second-order superlattice on the first-order superlattice:
[0082] 7.2.1) A yttrium source with a flow rate of 50 sccm and an aluminum source with a flow rate of 300 sccm are introduced into the reaction chamber to grow a 6 nm thick Y layer on the first-order superlattice. 0.2 Al 0.8 N layers;
[0083] 7.2.2) A gallium source with a flow rate of 120 sccm and an aluminum source with a flow rate of 150 sccm are introduced into the reaction chamber. 0.2 Al 0.8 A 3nm thick Al layer is grown on the N layer. 0.3 Ga 0.7 N layers;
[0084] 7.2.3) Repeat 7.2.1) and 7.2.2) for 10 cycles to obtain a second-order superlattice;
[0085] 7.3) Using MOCVD method to grow the third-order superlattice on the second-order superlattice:
[0086] 7.3.1) A yttrium source with a flow rate of 50 sccm and an aluminum source with a flow rate of 300 sccm are introduced into the reaction chamber to grow a 6 nm thick Y layer on the second-order superlattice. 0.2 Al 0.8 N layers;
[0087] 7.3.2) A gallium source with a flow rate of 150 sccm and an aluminum source with a flow rate of 60 sccm are introduced into the reaction chamber. 0.2 Al 0.8 A 3nm thick Al layer is grown on the N layer. 0.1 Ga 0.9 N layers;
[0088] 7.3.3) Repeat 7.3.1) and 7.3.2) for 10 cycles to obtain a third-order superlattice;
[0089] At this point, the epitaxy of the three-step stepped YAlN / AlGaN superlattice p-type layer 7 is completed.
[0090] Step eight, epitaxial ohmic contact layer, such as Figure 3 (g) as shown.
[0091] The reaction chamber temperature was maintained at 1050° C., the reaction chamber pressure was maintained at 30 Torr, and a nitrogen source with a flow rate of 2500 sccm, a gallium source with a flow rate of 150 sccm, and a magnesium source with a flow rate of 200 sccm were introduced at the same time, and a GaN ohmic contact layer 8 with a thickness of 10 nm was grown on the p-type layer by MOCVD method.
[0092] Step nine, etching the horizontal structure, such as Figure 3 (h) shown.
[0093] The ohmic contact layer is etched by dry etching with an etching depth of 887 nm. The etching is stopped in the middle of the n-type layer. The etching shape is a sector with a central angle of 90°.
[0094] Step 10, depositing electrodes, such as Figure 3 (i) as shown.
[0095] The temperature of the reaction chamber is maintained at 1200°C, and annealing is carried out for 10 minutes in a H2 atmosphere. Metal is deposited on the unetched ohmic contact layer to form a p-electrode, and metal is deposited on the etched n-type layer to form an n-electrode by sputtering, thereby completing the production of a deep ultraviolet LED device with a light emission wavelength of 280nm.
[0096] Example 2: Manufacturing a deep ultraviolet light emitting diode with a light emission wavelength of 255nm.
[0097] Step 1: pre-treating the substrate.
[0098] The specific implementation of this step is the same as step 1 of Example 1.
[0099] Step 2, epitaxial nucleation layer, such as Figure 3 (a) shown.
[0100] The temperature of the reaction chamber was raised to 1300° C., the pressure of the reaction chamber was maintained at 60 Torr, and a nitrogen source with a flow rate of 3000 sccm and an aluminum source with a flow rate of 30 sccm were introduced at the same time. A high-temperature AlN nucleation layer 2 with a thickness of 25 nm was grown on the c-plane sapphire substrate using the MOCVD method.
[0101] Step 3, epitaxial buffer layer, such as Figure 3 (b) as shown.
[0102] The temperature of the reaction chamber was maintained at 1300° C., the pressure of the reaction chamber was maintained at 60 Torr, and a nitrogen source with a flow rate of 3000 sccm and an aluminum source with a flow rate of 30 sccm were introduced at the same time. An AlN buffer layer 3 with a thickness of 1.5 μm was grown on the nucleation layer by MOCVD method.
[0103] Step 4, epitaxial n-type layer, such as Figure 3 (c) as shown.
[0104] The temperature of the reaction chamber was lowered to 1200°C, the pressure of the reaction chamber was maintained at 60 Torr, and a nitrogen source with a flow rate of 3000 sccm, a gallium source with a flow rate of 30 sccm, an aluminum source with a flow rate of 120 sccm, and a silicon source with a flow rate of 30 sccm were introduced at the same time. The MOCVD method was used to grow an n-type Al with a thickness of 2 μm on the buffer layer. 0.8 Ga 0.2 N-layer 4.
[0105] Step 5, epitaxial multi-quantum well layer, such as Figure 3 (d) as shown.
[0106] The reaction chamber temperature was maintained at 1200°C, the reaction chamber pressure was maintained at 60 Torr, and a nitrogen source with a flow rate of 3000 sccm was introduced. Five cycles of Al were grown on the n-type layer using the MOCVD method. 0.6 Ga 0.4 N / A 0.75 Ga 0.25 N multi-quantum well layer 5, that is, firstly introduce a gallium source with a flow rate of 40sccm and an aluminum source with a flow rate of 130sccm, and grow an Al layer with a thickness of 10nm on the n-type layer. 0.75 Ga 0.25 N quantum barrier layer; then introduce a gallium source with a flow rate of 60sccm and an aluminum source with a flow rate of 120sccm to grow a 2nm thick Al layer on the quantum barrier layer 0.6 Ga 0.4 N quantum well layers; five cycles of alternating growth are performed to obtain a multi-quantum well layer.
[0107] Step 6, epitaxial electron blocking layer, such as Figure 3 (e) as shown.
[0108] The temperature of the reaction chamber was raised to 1250°C, the pressure of the reaction chamber was maintained at 60 Torr, and a nitrogen source with a flow rate of 2500 sccm, a gallium source with a flow rate of 15 sccm, and an aluminum source with a flow rate of 170 sccm were introduced at the same time. Al with a thickness of 25 nm was grown on the multi-quantum well layer using the MOCVD method. 0.95 Ga 0.05 N electron blocking layer 6.
[0109] Step 7, epitaxial p-type layer, such as Figure 3 (f) as shown.
[0110] The temperature of the reaction chamber was lowered to 1200°C, the pressure of the reaction chamber was maintained at 60 Torr, a nitrogen source with a flow rate of 3000 sccm and a magnesium source with a flow rate of 300 sccm were introduced at the same time, and then a three-step ladder superlattice was grown according to the following process conditions:
[0111] 7a) The first-order superlattice is grown on the electron blocking layer by using the MOCVD method. That is, a yttrium source with a flow rate of 60 sccm and an aluminum source with a flow rate of 280 sccm are first introduced, and a layer of Y with a thickness of 5 nm is grown on the electron blocking layer. 0.3 Al 0.7 N layer; then introduce a gallium source with a flow rate of 60sccm and an aluminum source with a flow rate of 120sccm, 0.3 Al 0.7 A 2nm thick Al layer is grown on the N layer. 0.6 Ga 0.4 N layers; repeat this process for 8 cycles to obtain the first-order superlattice;
[0112] 7b) A second-order superlattice is grown on the first-order superlattice by MOCVD, that is, a yttrium source with a flow rate of 60 sccm and an aluminum source with a flow rate of 280 sccm are introduced first, and a layer of Y with a thickness of 5 nm is grown on the first-order superlattice. 0.3 Al 0.7 N layer; then introduce a gallium source with a flow rate of 130sccm and an aluminum source with a flow rate of 150sccm, 0.3 Al 0.7 A 2nm thick Al layer is grown on the N layer. 0.4 Ga 0.6 N layers; repeat this process for 8 cycles to obtain the second-order superlattice;
[0113] 7c) A third-order superlattice is grown on the second-order superlattice by MOCVD, that is, a yttrium source with a flow rate of 60 sccm and an aluminum source with a flow rate of 280 sccm are first introduced, and a layer of Y with a thickness of 5 nm is grown on the second-order superlattice. 0.3 Al 0.7 N layer; then introduce a gallium source with a flow rate of 180sccm and an aluminum source with a flow rate of 120sccm, 0.3 Al 0.7 A 2nm thick Al layer is grown on the N layer. 0.2 Ga 0.8 N layers; repeat this process for 8 cycles to obtain the third-order superlattice;
[0114] At this point, the epitaxy of the three-step stepped YAlN / AlGaN superlattice p-type layer 7 is completed.
[0115] Step 8, epitaxial ohmic contact layer, such as Figure 3 (g) as shown.
[0116] The temperature of the reaction chamber is maintained at 1200° C., the pressure of the reaction chamber is maintained at 60 Torr, and a nitrogen source with a flow rate of 3000 sccm, a gallium source with a flow rate of 240 sccm, and a magnesium source with a flow rate of 300 sccm are introduced at the same time, and a GaN ohmic contact layer 8 with a thickness of 15 nm is grown on the p-type layer by MOCVD method.
[0117] Step 9, etching the horizontal structure, such as Figure 3 (h) shown.
[0118] The ohmic contact layer is etched by dry etching with an etching depth of 813 nm. The etching is stopped in the middle of the n-type layer. The etching shape is a sector with a central angle of 90°.
[0119] Step 10, depositing electrodes, such as Figure 3 (i) as shown.
[0120] The specific completion of this step is the same as step ten of Example 1, and the production of a deep ultraviolet LED device with a light emission wavelength of 255 nm is completed.
[0121] Example 3: Manufacturing a deep ultraviolet light emitting diode with a light emission wavelength of 227nm.
[0122] In step A, the substrate is pretreated.
[0123] The specific implementation of this step is the same as step 1 of Example 1.
[0124] Step B, epitaxial nucleation layer, such as Figure 3 (a) shown.
[0125] The temperature of the reaction chamber was raised to 1350° C., the pressure of the reaction chamber was raised to 100 Torr, and a nitrogen source with a flow rate of 4000 sccm and an aluminum source with a flow rate of 40 sccm were introduced at the same time. A high-temperature AlN nucleation layer 2 with a thickness of 15 nm was grown on the c-plane sapphire substrate using the MOCVD method.
[0126] Step C, epitaxial buffer layer, such as Figure 3 (b) as shown.
[0127] The temperature of the reaction chamber was maintained at 1350° C., the pressure of the reaction chamber was maintained at 100 Torr, and a nitrogen source with a flow rate of 4000 sccm and an aluminum source with a flow rate of 40 sccm were introduced at the same time, and an AlN buffer layer 3 with a thickness of 2 μm was grown on the nucleation layer by MOCVD method.
[0128] Step D, epitaxially growing an n-type layer, such as Figure 3 (c) as shown.
[0129] The reaction chamber temperature was maintained at 1350°C, the reaction chamber pressure was maintained at 100 Torr, and a nitrogen source with a flow rate of 4000 sccm, a gallium source with a flow rate of 50 sccm, an aluminum source with a flow rate of 180 sccm, and a silicon source with a flow rate of 50 sccm were introduced at the same time. An n-type Al with a thickness of 2.5 μm was grown on the buffer layer by MOCVD method. 0.9 Ga 0.1 N-layer 4.
[0130] Step E, epitaxial multi-quantum well layer, such as Figure 3 (d) as shown.
[0131] The reaction chamber temperature was maintained at 1350°C, the reaction chamber pressure was maintained at 100 Torr, and a nitrogen source with a flow rate of 4000 sccm was introduced. Five cycles of Al were grown on the n-type layer using the MOCVD method. 0.79 Ga 0.21 N and Al 0.87 Ga 0.13 N multi-quantum well layer 5:
[0132] E1) A gallium source with a flow rate of 40 sccm and an aluminum source with a flow rate of 170 sccm are introduced to grow an Al layer with a thickness of 7 nm on the n-type layer. 0.87 Ga 0.13 N quantum barrier layer
[0133] E2) A gallium source with a flow rate of 60 sccm and an aluminum source with a flow rate of 180 sccm are introduced to grow an Al layer with a thickness of 1.3 nm on the quantum barrier layer. 0.79 Ga 0.21 N quantum well layer
[0134] E3) Repeat E1) and E2) for five cycles of alternating growth to obtain a multi-quantum well layer.
[0135] Step F, epitaxial electron blocking layer, such as Figure 3 (e) as shown.
[0136] The temperature of the reaction chamber was raised to 1400°C, the pressure of the reaction chamber was maintained at 100 Torr, and a nitrogen source with a flow rate of 4000 sccm, a gallium source with a flow rate of 10 sccm, and an aluminum source with a flow rate of 180 sccm were introduced at the same time. Al with a thickness of 20 nm was grown on the multi-quantum well layer using the MOCVD method. 0.98 Ga 0.02 N electron blocking layer 6.
[0137] Step G, epitaxial p-type layer, such as Figure 3 (f) as shown.
[0138] The temperature of the reaction chamber was lowered to 1350°C, the pressure of the reaction chamber was maintained at 100 Torr, a nitrogen source with a flow rate of 4000 sccm and a magnesium source with a flow rate of 400 sccm were introduced at the same time, and then a three-step ladder superlattice was grown according to the following process conditions:
[0139] G1) The first-order superlattice is grown on the electron blocking layer using the MOCVD method:
[0140] G1.1) A yttrium source with a flow rate of 80 sccm and an aluminum source with a flow rate of 280 sccm are introduced into the reaction chamber to grow a 7 nm thick Y layer on the electron blocking layer. 0.4 Al 0.6 N layers;
[0141] G1.2) A gallium source with a flow rate of 60 sccm and an aluminum source with a flow rate of 150 sccm are introduced into the reaction chamber. 0.4 Al 0.6 A 4nm thick Al layer is grown on the N layer. 0.8 Ga 0.2 N layers;
[0142] G1.3) Repeat G1.1) and G1.2) for 7 cycles to obtain the first-order superlattice;
[0143] G2) A second-order superlattice is grown on the first-order superlattice using the MOCVD method:
[0144] G2.1) A yttrium source with a flow rate of 80 sccm and an aluminum source with a flow rate of 280 sccm are introduced into the reaction chamber to grow a layer of Y with a thickness of 7 nm on the first-order superlattice. 0.4 Al 0.6 N layers;
[0145] G2.2) A gallium source with a flow rate of 80 sccm and an aluminum source with a flow rate of 120 sccm are introduced into the reaction chamber. 0.4 Al 0.6 A 4nm thick Al layer is grown on the N layer. 0.5 Ga 0.5 N layers;
[0146] G2.3) Repeat G2.1) and G2.2) for 7 cycles to obtain a second-order superlattice;
[0147] G3) Growing a third-order superlattice on the second-order superlattice using the MOCVD method:
[0148] G3.1) A yttrium source with a flow rate of 80 sccm and an aluminum source with a flow rate of 280 sccm are introduced into the reaction chamber to grow a 7 nm thick Y layer on the second-order superlattice. 0.4 Al 0.6 N layers;
[0149] G3.2) A gallium source with a flow rate of 120 sccm and an aluminum source with a flow rate of 100 sccm are introduced into the reaction chamber. 0.4 Al 0.6 A 4nm thick Al layer is grown on the N layer. 0.3 Ga 0.7 N layers;
[0150] G.3.3) Repeat G3.1) and G3.2) for 7 cycles to obtain a third-order superlattice;
[0151] At this point, the epitaxy of the three-step stepped YAlN / AlGaN superlattice p-type layer 7 is completed.
[0152] Step H, epitaxial ohmic contact layer, such as Figure 3 (g) as shown.
[0153] The reaction chamber temperature was maintained at 1350° C., the reaction chamber pressure was maintained at 100 Torr, and a nitrogen source with a flow rate of 4000 sccm, a gallium source with a flow rate of 300 sccm, and a magnesium source with a flow rate of 400 sccm were introduced at the same time, and a GaN ohmic contact layer 8 with a thickness of 20 nm was grown on the p-type layer by MOCVD method.
[0154] Step I, etching the horizontal structure, such as Figure 3 (h) shown.
[0155] The ohmic contact layer is etched by dry etching with an etching depth of 778 nm. The etching is stopped in the middle of the n-type layer. The etching shape is a sector with a central angle of 90°.
[0156] Step J, depositing electrodes, such as Figure 3 (i) as shown.
[0157] The specific completion of this step is the same as step ten of Example 1, and the production of a deep ultraviolet LED device with a light emission wavelength of 227nm is completed.
[0158] The above descriptions are only three specific examples of the present invention and do not constitute any limitation to the present invention. Obviously, for professionals in this field, after understanding the content and principles of the present invention, it is possible to make various modifications and changes in form and details without departing from the principles and structures of the present invention. However, these modifications and changes based on the ideas of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A high-efficiency deep ultraviolet light-emitting diode with a stepped composition YAlN / AlGaN superlattice p-type layer, which comprises from bottom to top: A substrate (1), a nucleation layer (2), a buffer layer (3), an n-type layer (4), a multi-quantum well layer (5), an electron blocking layer (6), a p-type layer (7), and an ohmic contact layer (8), characterized in that: The p-type layer (7) adopts a three-step stepped component YAlN / AlGaN superlattice, and the parameters of each step are as follows: The number of first-order superlattice periods is 7-10, the Al component of YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of AlGaN material in each period ranges from 0.5-0.8, the thickness is 1nm-4nm; The number of periods of the second-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.3-0.5, the thickness is 1nm-4nm; The number of periods of the third-order superlattice is 7-10, the Al component of the YAlN material in each period ranges from 0.6-0.8, the thickness is 3nm-7nm, and the Al component of the AlGaN material in each period ranges from 0.1-0.3, the thickness is 1nm-4nm; The Al component of the AlGaN material in the three stages decreases gradually, forming a YAlN / AlGaN superlattice p-type layer with a stepped composition, so as to effectively improve the luminous efficiency of the device.
2. The diode according to claim 1, characterized in that: The multi-quantum well layer (5) comprises five periods of quantum wells and quantum barriers, wherein the quantum wells of each period are made of AlGaN material with a thickness of 1.3nm-3nm and an Al component of 0.4-0.79, and the quantum barriers of each period are made of AlGaN material with a thickness of 7nm-12nm and an Al component of 0.5-0.
87.
3. The diode according to claim 1, characterized in that: The substrate (1) is made of c-plane sapphire material; The nucleation layer (2) is made of high-temperature AlN material with a thickness of 15nm-35nm; The buffer layer (3) is made of AlN material with a thickness of 1 μm-2 μm; The ohmic contact layer (8) is made of GaN material with a thickness of 10nm-20nm.
4. The diode according to claim 1, characterized in that: The n-type layer (4) is made of AlGaN material with a thickness of 1.5 μm-2.5 μm and an Al component of 0.6-0.9; The electron blocking layer (6) is made of AlGaN material with a thickness of 20nm-30nm and an Al component of 0.65-0.
98.
5. A method for manufacturing a high-efficiency deep ultraviolet light-emitting diode of a YAlN / AlGaN superlattice p-type layer, characterized in that The steps include: 1) Pre-treating the substrate (1) by cleaning and nitridation; 2) growing a nucleation layer (2) of 15 nm to 35 nm on the pretreated substrate using a MOCVD process; 3) growing a buffer layer (3) with a thickness of 1 μm to 2 μm on the nucleation layer by using a MOCVD process; 4) growing an n-type layer (4) with a thickness of 1.5 μm to 2.5 μm on the buffer layer by using a MOCVD process; 5) on the n-type layer, growing a multi-quantum well layer (5) including five periods of quantum wells and quantum barriers by MOCVD process, wherein the thickness of the quantum wells in each period is 1.3 nm to 3 nm, and the thickness of the quantum barriers in each period is 7 nm to 12 nm; 6) growing an electron blocking layer (6) with a thickness of 20 nm to 30 nm on the multi-quantum well layer by using a MOCVD process; 7) On the electron blocking layer, a three-step stepped YAlN / AlGaN superlattice p-type layer with decreasing Al composition is grown by MOCVD process (7): 7a) growing a first-order superlattice with a period of 7-10 on the electron blocking layer by MOCVD process, wherein the thickness of the YAlN material in each period of the first-order superlattice is 3nm-7nm, the thickness of the AlGaN material in each period is 1nm-4nm, and the Al component range is 0.5-0.8; 7b) growing a second-order superlattice with a period of 7-10 on the first-order superlattice by MOCVD process, wherein the thickness of the YAlN material of each period of the second-order superlattice is 3nm-7nm, the thickness of the AlGaN material of each period is 1nm-4nm, and the Al composition ranges from 0.3 to 0.5; 7c) growing a third-order superlattice with a period of 7-10 on the second-order superlattice by MOCVD process, wherein the thickness of the YAlN material of each period of the third-order superlattice is 3nm-7nm, the thickness of the AlGaN material of each period is 1nm-4nm, and the Al composition ranges from 0.1 to 0.3; 8) On the p-type layer, an ohmic contact layer (8) with a thickness of 10 nm to 20 nm is grown by MOCVD process; 9) The ohmic contact layer is etched by dry etching, the etching depth is from the surface to the middle of the n-type layer, and the etching shape is a sector with a central angle of 90°; 10) Using a metal sputtering method, metal is deposited on the unetched ohmic contact layer to form a p-electrode, and using a metal sputtering method, metal is deposited on the etched n-type layer to form an n-electrode, thereby completing the production of the LED.
6. The method according to claim 5, characterized in that The MOCVD process used in step 2) and step 3) is to set the following condition parameters for the reaction chamber: The reaction chamber temperature is 1250-1350°C, The reaction chamber pressure is maintained at 30-100 Torr. A nitrogen source with a flow rate of 2000-4000 sccm and an aluminum source with a flow rate of 20-40 sccm are introduced into the reaction chamber.
7. The method according to claim 5, characterized in that The MOCVD process used in step 4) is to set the following condition parameters for the reaction chamber: The reaction chamber temperature is 1150-1350°C, The reaction chamber pressure is maintained at 20-100 Torr. A nitrogen source with a flow rate of 2500-4000 sccm, a gallium source with a flow rate of 30-60 sccm, an aluminum source with a flow rate of 120-180 sccm, and a silicon source with a flow rate of 30-50 sccm are introduced into the reaction chamber.
8. The method according to claim 5, characterized in that The MOCVD process used in step 5) is to set the following condition parameters for the reaction chamber: The reaction chamber temperature is 1150-1350°C, The reaction chamber pressure is maintained at 20-100 Torr. A nitrogen source with a flow rate of 2500-4000 sccm, a gallium source with a flow rate of 40-120 sccm, and an aluminum source with a flow rate of 120-180 sccm are introduced into the reaction chamber.
9. The method according to claim 5, characterized in that The MOCVD process conditions used in step 7 are as follows: The temperature, pressure and gas of 7a), 7b) and 7c) are the same, that is, the temperature of the reaction chamber is 1050-1350°C, the pressure of the reaction chamber is maintained at 30-100Torr, the gases introduced are nitrogen source, gallium source, aluminum source, yttrium source and magnesium source, and the flow rate of the nitrogen source is 2500-4000sccm, the flow rate of the yttrium source is 50-80sccm, and the flow rate of the magnesium source is 200-400sccm; The flow rates of the gallium source and the aluminum source in 7a), 7b) and 7c) are different, namely: In step 7a), a gallium source flow rate of 60-150 sccm and an aluminum source flow rate of 120-320 sccm are introduced into the reaction chamber; In step 7b), a gallium source flow rate of 80-130 sccm and an aluminum source flow rate of 120-300 sccm are introduced into the reaction chamber; In step 7c), the gallium source flow rate is 120-180 sccm and the aluminum source flow rate is 60-300 sccm into the reaction chamber.
10. The method according to claim 5, characterized in that: The MOCVD process used in step 6) is to set the reaction chamber temperature to 1200-1400° C., maintain the reaction chamber pressure at 30-100 Torr, and introduce a nitrogen source with a flow rate of 1800-4000 sccm, a gallium source with a flow rate of 10-50 sccm, and an aluminum source with a flow rate of 120-180 sccm into the reaction chamber; The MOCVD process used in step 8) is to set the reaction chamber temperature to 1050-1350°C, maintain the reaction chamber pressure at 20-100Torr, and introduce a nitrogen source with a flow rate of 2500-4000sccm, a gallium source with a flow rate of 150-300sccm, and a magnesium source with a flow rate of 200-400sccm into the reaction chamber.
Citation Information
Patent Citations
Method of adopting MOCVD technology to prepare deep ultraviolet LED
CN105161582A
Method for preparing p-type AlGaN / AlInGaN electron blocking layer near ultraviolet LED with doping density and Al component in stepwise change
CN106299038A
Semiconductor Heterostructure with P-type Superlattice
US20190103509A1
High electron mobility transistor (HEMT) device
US20190237570A1