Heat insulation coating and preparation method thereof
Through the multi-layer structural design of Pt-Al2O3/Cr2O3/TiO2 composite coating, the corrosion and coating bonding problems of high-temperature containers in harsh environments are solved, and the efficient heat insulation and heat resistance are improved, and the coating is extended The service life and improves mechanical properties.
Patent Information
- Application Number
- CN202411066637.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Existing high-temperature and high-pressure containers are easily corroded in harsh environments. The interface structure difference between the thermal barrier coating and the high-temperature resistant superalloy matrix leads to insufficient compatibility and binding force, resulting in early fall of the coating and high-temperature alloys being coated. The mechanical properties deteriorate during layer deposition.
Using Pt-Al2O3/Cr2O3/TiO2 composite coating and its preparation method, the multi-layer composite structure utilizes the low thermal conductivity of oxides and the chemical stability of the platinum layer, and combines the dense structure of Cr and Al to form high-efficiency heat insulation and resistance Coatings with thermal corrosion and thermal shock.
It improves the overall thermal insulation and high-temperature oxidation resistance of the coating, enhances the binding force with the high-temperature alloy matrix, extends the service life of the coating, and improves the hardness and impact resistance of the coating.
Smart Images

Figure CN118957582A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal insulation coatings deposited on surfaces of metal materials, and specifically relates to a thermal insulation coating and a preparation method thereof, and in particular to a Pt-Al2O3 / Cr2O3 / TiO2 composite coating and a preparation method thereof. Background Art
[0002] The operating environment of high-temperature and high-pressure vessels frequently used in the coal chemical industry, such as coking furnaces, combustion furnaces, oxidation furnaces, or gasification furnaces, is usually a high-temperature and corrosive environment. This harsh environment causes great damage to the internal structure of the container, especially the heated inner wall surface. In order to protect such high-temperature and high-pressure equipment from the erosion of the above-mentioned high-temperature and corrosive environment and to extend the service life of the equipment, people have come up with many ways and countermeasures.
[0003] For example, people use high-temperature resistant superalloys containing metal elements such as Ni, Co, and W as mentioned in the patent publication number "CN102639283B" as materials for manufacturing such equipment. Such alloys have high mechanical strength at high temperatures, and their heat resistance is improved by adding elements such as Cr, Al, and / or Si. These elements can form oxide films in an oxidizing atmosphere, thereby providing good protection for the above-mentioned high-temperature resistant superalloy components.
[0004] Another method is to apply thermal barrier coating (TBC), especially ceramic thermal barrier coating, on the surface of components subjected to high temperature and corrosive environment to physically isolate and protect the above-mentioned high temperature superalloys. However, due to the different interface structures between thermal barrier coating and high temperature superalloy, the physical and chemical properties of the two are very different. Under the adverse effects of thermal attraction generated by temperature gradient and various high temperature erosion or penetration, they cannot achieve good compatibility and strong bonding. As a result, the thermal barrier coating falls off or peels off from the surface of the high temperature superalloy substrate prematurely. In order to solve this problem, it is usually necessary to implant a bonding coating, usually an intermetallic compound, between the interface of the thermal barrier coating and the high temperature superalloy substrate to increase the compatibility and bonding strength of the two.
[0005] In addition, in some engines or gas turbine hot end parts, they are often subjected to high temperature and thermal corrosion environments, and the requirements for materials are getting higher and higher. For example, nickel-based high-temperature alloys are the most commonly used materials for aircraft engine blades. They are at extremely high temperatures during service. In order to ensure that the high-temperature alloys are not oxidized during use, a layer of high-Al content anti-oxidation coating, also known as a metal bonding layer, is often prepared on its surface. By forming a dense aluminum oxide film at high temperature, the high-temperature alloy substrate is protected. High-temperature anti-oxidation coatings generally include cladding MCrAlY coatings (M = Ni, Co or Ni + Co) and PtAl diffusion coatings. The alloy surface temperature is usually low during the deposition process of the cladding coating. In order to ensure the bonding strength between the coating and the alloy, high-temperature diffusion treatment is required; the diffusion coating needs to undergo high-temperature diffusion and deposition steps during the preparation process. After the coating is deposited, the substrate and the coating have a high bonding strength. However, during the high-temperature deposition / diffusion process of the coating preparation, the high-temperature alloy substrate structure will evolve, which will cause the mechanical properties of the high-temperature alloy to decrease, which is not conducive to the application of high-temperature alloys.
[0006] Therefore, developing a composite coating that has both good thermal insulation properties and good resistance to heat corrosion and thermal shock is an important way to solve the above problems. Summary of the invention
[0007] In order to address the defects in the prior art, the present invention proposes a thermal insulation coating and a preparation method thereof, the purpose of which is to provide a Pt-Al2O3 / Cr2O3 / TiO2 composite coating as a thermal insulation coating which has thermal insulation properties and good resistance to heat corrosion and thermal shock and a preparation method thereof.
[0008] The present invention utilizes the following technical solutions.
[0009] A method for preparing a thermal insulation coating, comprising:
[0010] Step 1: Pre-cleaning of workpiece;
[0011] Step 2: Plating a transition layer on the pre-cleaned workpiece;
[0012] Step 3: Plating a CrON / AlCrON intermediate layer on the workpiece after the transition layer is plated;
[0013] Step 4: Plating the workpiece after plating the CrON / AlCrON intermediate layer with an AlCrTi / Al2O3 / Cr2O3 / TiO2 layer;
[0014] Step 5: After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source in the vacuum chamber, stop the gas supply, continue to evacuate the vacuum chamber, cool it to below 100°C with the furnace, open the vacuum chamber, and take out the workpiece processed in step 5;
[0015] Step 6: Plate a Pt layer on the workpiece processed in step 5.
[0016] Furthermore, step 1 specifically includes: after grinding and sandblasting the surface of the workpiece, ultrasonically treating the workpiece in an alcohol solution for 10 to 20 minutes, drying the workpiece with hot air, and then placing the workpiece on a workpiece rack in a vacuum chamber to wait for coating.
[0017] Furthermore, step 2 specifically includes: using a high-purity aluminum-chromium target arc source in a vacuum chamber, when the vacuum degree in the vacuum chamber reaches 1×10 -3 Pa~1×10 -2 When the temperature reaches 0.0400°C, the workpiece holder is turned on and the rotation speed is adjusted to 1-4 rpm, and the vacuum chamber is heated to 300-500°C; argon gas is introduced into the vacuum chamber, and the gas pressure is controlled between 0.3 and 6 Pa; the pre-cleaned workpiece, that is, the substrate, is subjected to a pulsed negative bias voltage in the range of -50 to -600 V, and the arc enhanced glow discharge ion source is turned on and the gas is glow discharged, and the pre-cleaned workpiece, that is, the sample, is glow cleaned for 20 to 60 minutes; the argon gas flow rate is adjusted so that the vacuum chamber pressure is 0.02 to 1.0 Pa, and the high-purity aluminum chromium The target arc source has an arc current of 50 to 200A, the pulse negative bias is adjusted to -50V to -500V, the duty cycle of the pulse negative bias is adjusted to 20% to 80%, and the transition layer formed by the AlCr layer is deposited for 5 to 40 minutes; then nitrogen is introduced into the vacuum chamber, the gas pressure is adjusted to 0.5 to 5.0Pa, the pure chromium target and the high-purity aluminum-chromium alloy target arc source are turned on, the arc current is 50 to 200A, the pulse negative bias is adjusted to -50V to -500V, the duty cycle of the pulse negative bias is adjusted to 20% to 80%, and the transition layer formed by the CrN / AlCrN layer is deposited for 4 to 40 minutes.
[0018] Furthermore, step 3 specifically includes: using a chromium target and an aluminum-chromium alloy target, adjusting the argon pressure in the vacuum chamber to 0.1-0.5 Pa, introducing nitrogen and oxygen, with the nitrogen and oxygen flow ratio in the range of 2:1-1:2, and controlling the pressure at 0.2-1.5 Pa, applying a pulsed negative bias voltage of -50V to -300V to the workpiece after the transition layer is plated, that is, substrate 2, with a pulsed negative bias duty cycle of 20% to 80%, and turning on the arc enhanced glow discharge ion source; adjusting the arc current of the chromium target and the aluminum-chromium alloy target to 50-200A, and the deposition time to 5-20 minutes.
[0019] Furthermore, step 4 specifically includes:
[0020] Step 4-1: Using aluminum-chromium and aluminum-titanium alloy targets, adjusting the argon gas pressure in the vacuum chamber to 0.1-2 Pa, applying a pulsed negative bias voltage of -50V to -300V to the workpiece after the CrON / AlCrON intermediate layer is plated, that is, the substrate three, and the pulsed negative bias voltage duty cycle is 20% to 80%, turning on the arc enhanced glow discharge ion source; adjusting the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50-200A, and the deposition time to 1 to 10 minutes;
[0021] Step 4-2: Then, oxygen is introduced into the vacuum chamber, and the vacuum chamber pressure is adjusted to 0.2-2.0 Pa. A pulsed negative bias voltage of -50V--300V is applied to the substrate three, and the pulsed negative bias voltage duty ratio is 20%-80%, and the arc enhanced glow discharge ion source is turned on; the target arc current of aluminum-chromium and aluminum-titanium alloy is adjusted to 50-200A, and the deposition time is 1-10 minutes;
[0022] Step 4-3: Repeat steps 4-1 to 4-2 for 10 to 50 times, and the total deposition time is controlled within 30 to 300 minutes;
[0023] Step 4-4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure in the vacuum chamber to 0.1~2Pa, apply a pulsed negative bias voltage of -50V~-300V to the substrate three, and the pulsed negative bias duty cycle is 20%~80%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50~200A, and the deposition time is 10~30 minutes.
[0024] Furthermore, step 6 specifically includes:
[0025] The surface of the workpiece taken out after being processed in step 5 is polished, and then the surface of the workpiece treated in step 5 is electroplated with platinum.
[0026] Further, the method for electroplating platinum includes: using [Pt(NH3)2(NO2)2] plating solution, the current density during electroplating is 0.4A / dm 2 ~5A / dm 2 The thickness of the platinum coating obtained is 2 to 10 microns.
[0027] A thermal insulation coating, comprising:
[0028] On the substrate surface from bottom to top are the bonding layer formed by the AlCr layer, the transition layer formed by the CrN / AlCrN layer, the intermediate layer formed by the CrON / AlCrON layer, the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer. The thermal insulation coating is also the Pt-Al2O3 / Cr2O3 / TiO2 composite coating.
[0029] Furthermore, the thicknesses of the bonding layer formed by the AlCr layer, the transition layer formed by the CrN / AlCrN layer, the intermediate layer formed by the CrON / AlCrON layer, the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer are 1 to 10.0 microns, 1 to 10.0 microns, 1 to 10.0 microns, 5 to 60.0 microns and 3 to 10.0 microns, respectively.
[0030] Furthermore, in the bonding layer formed by the AlCr layer, the Al content is 50-70 at.%; in the transition layer formed by the CrN / AlCrN layer, the Al content in the AlCrN layer is 50-70 at.%; in the intermediate layer formed by the CrON / AlCrON layer, the O content in the CrON layer is 10-20 at.%, and the N content is 20-30 at.%, the Al content in the AlCrON layer is 50-70 at.%, the O content is 10-20 at.%, and the N content is 20-30 at.%; in the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating, the Al content in the AlCrTi layer is 50-70 at.%; in the Al2O3 / Cr2O3 / TiO2 layer, the Al2O3 content is 50-70 at.%, the Cr2O3 content is 20-40 at.%, and the TiO2 content is 5-20 at.%.
[0031] The beneficial effects of the present invention are that, compared with the prior art, the technical effects of the present invention include:
[0032] 1. The present invention adopts a multi-layer composite thermal insulation coating, utilizing the characteristics of the oxide coating, such as low thermal conductivity, high heat resistance temperature, resistance to high-temperature oxidation and heat corrosion, and utilizing the characteristics of the platinum coating, such as good chemical stability, promotion of selective oxidation of aluminum and favorability to form a purer and better-bonded Al2O3 coating. It can better bring into play the technical advantages of various coatings and has a significant promoting effect on promoting the improvement of the overall thermal insulation and high-temperature oxidation resistance of the composite coating.
[0033] 2. The present invention selects a composite target of Cr and Al. In the process of generating the Al2O3 coating, the nucleation of Cr2O3 is more conducive to the nucleation and growth of the dense structure α-Al2O3 phase, which promotes the compactness of the overall structure of the coating; and the dense structure α-Al2O3 phase is conducive to improving the high-temperature oxidation resistance of the coating, and the Cr2O3 coating is conducive to improving the heat corrosion resistance of the coating. The combination of the two is conducive to improving the overall high-temperature oxidation resistance and heat corrosion resistance of the coating.
[0034] 3. The present invention deposits the AlCrTi layer before depositing the Pt layer, which is beneficial to promoting the oxidation of the AlCrTi layer and the formation of a dense alumina layer during service, and is more conducive to giving full play to the respective advantages of Pt and Al2O3 and promoting the improvement of the overall performance of the coating.
[0035] 4. The present invention is completed by ion beam assisted arc ion plating technology. This method not only has a faster deposition rate, but also has fewer large particles on the surface of the prepared composite coating, and the coating is more dense. In addition to having good thermal insulation properties, the coating also has the advantages of high hardness, impact resistance and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic structural diagram of the thermal insulation coating in the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the following will be combined with the drawings in the embodiments of the present invention to clearly and completely express the technical solution of the present invention. The embodiments expressed in this application are only some embodiments of the present invention, not all embodiments. According to the spirit of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the protection scope of the present invention.
[0038] A method for preparing a thermal insulation coating according to the present invention comprises:
[0039] Step 1: Pre-cleaning of workpiece;
[0040] In a preferred but non-limiting embodiment of the present invention, step 1 specifically includes: grinding and sandblasting the workpiece surface, ultrasonically treating the workpiece in an alcohol solution for 10 to 20 minutes, drying the workpiece with hot air, and loading the workpiece onto a workpiece rack in a vacuum chamber to wait for coating. The workpiece here may be a high temperature alloy or a superalloy. The alcohol solution may be an alcohol solution with a mass concentration of 70% to 90%.
[0041] Step 2: Plating a transition layer on the pre-cleaned workpiece;
[0042] In a preferred but non-limiting embodiment of the present invention, step 2 specifically comprises: using a high-purity aluminum-chromium target arc source disposed in a vacuum chamber, when the vacuum degree in the vacuum chamber reaches 1×10 -3 Pa~1×10 -2When the temperature reaches 0.0400°C, the workpiece holder is turned on and the rotation speed is adjusted to 1-4 rpm, and the vacuum chamber is heated to 300-500°C; argon gas is introduced into the vacuum chamber, and the gas pressure is controlled between 0.3 and 6 Pa; the pre-cleaned workpiece, that is, the substrate, is subjected to a pulsed negative bias voltage in the range of -50 to -600 V, and the arc enhanced glow discharge ion source is turned on and the gas is glow discharged, and the pre-cleaned workpiece, that is, the sample, is glow cleaned for 20 to 60 minutes; the argon gas flow rate is adjusted so that the vacuum chamber pressure is 0.02 to 1.0 Pa, and the high-purity aluminum chromium The target arc source has an arc current of 50 to 200A, a pulse negative bias voltage is adjusted to -50V to -500V, and a pulse negative bias voltage duty ratio is adjusted to 20% to 80%. The transition layer formed by the AlCr layer is deposited for 5 to 40 minutes. Then, nitrogen is introduced into the vacuum chamber, and the gas pressure is adjusted to 0.5 to 5.0Pa. The pure chromium target and the high-purity aluminum-chromium alloy target arc source are turned on, and the arc current is 50 to 200A. The pulse negative bias voltage is adjusted to -50V to -500V, and the pulse negative bias voltage duty ratio is adjusted to 20% to 80%. The transition layer formed by the CrN / AlCrN layer is deposited for 4 to 40 minutes. The purity of the high-purity aluminum-chromium target arc source is 99.95%. The pure chromium target arc source is also arranged in the hollow chamber.
[0043] Step 3: Plating a CrON / AlCrON intermediate layer on the workpiece after the transition layer is plated;
[0044] In a preferred but non-limiting embodiment of the present invention, step 3 specifically includes: using a chromium target and an aluminum-chromium alloy target, adjusting the argon pressure in the vacuum chamber to 0.1-0.5 Pa, introducing nitrogen and oxygen, the nitrogen and oxygen flow ratio is in the range of 2:1-1:2, the pressure is controlled at 0.2-1.5 Pa, and a pulse negative bias voltage of -50V to -300V is applied to the workpiece after the transition layer is plated, that is, the second substrate, and the pulse negative bias duty cycle is 20% to 80%, and the arc enhanced glow discharge ion source is turned on; the arc current of the chromium target and the aluminum-chromium alloy target is adjusted to 50-200A, and the deposition time is 5 to 20 minutes.
[0045] Step 4: Plating the workpiece after plating the CrON / AlCrON intermediate layer with an AlCrTi / Al2O3 / Cr2O3 / TiO2 layer;
[0046] In a preferred but non-limiting embodiment of the present invention, step 4 specifically comprises:
[0047] Step 4-1: Using aluminum-chromium and aluminum-titanium alloy targets, adjusting the argon gas pressure in the vacuum chamber to 0.1-2 Pa, applying a pulsed negative bias voltage of -50V to -300V to the workpiece after the CrON / AlCrON intermediate layer is plated, that is, the substrate three, and the pulsed negative bias voltage duty cycle is 20% to 80%, turning on the arc enhanced glow discharge ion source; adjusting the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50-200A, and the deposition time to 1 to 10 minutes;
[0048] Step 4-2: Then, oxygen is introduced into the vacuum chamber, and the vacuum chamber pressure is adjusted to 0.2-2.0 Pa. A pulsed negative bias voltage of -50V--300V is applied to the substrate three, and the pulsed negative bias voltage duty ratio is 20%-80%, and the arc enhanced glow discharge ion source is turned on; the target arc current of aluminum-chromium and aluminum-titanium alloy is adjusted to 50-200A, and the deposition time is 1-10 minutes;
[0049] Step 4-3: Repeat steps 4-1 to 4-2 for 10 to 50 times, and the total deposition time is controlled within 30 to 300 minutes;
[0050] Step 4-4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure in the vacuum chamber to 0.1~2Pa, apply a pulsed negative bias voltage of -50V~-300V to the substrate three, and the pulsed negative bias duty cycle is 20%~80%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50~200A, and the deposition time is 10~30 minutes.
[0051] Step 5: After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source in the vacuum chamber, stop the gas supply, continue to evacuate the vacuum chamber, cool it to below 100°C with the furnace, open the vacuum chamber, and take out the workpiece processed in step 5;
[0052] Step 6: Plate a Pt layer on the workpiece processed in step 5.
[0053] In a preferred but non-limiting embodiment of the present invention, step 6 specifically comprises:
[0054] The surface of the workpiece taken out after being processed in step 5 is polished, and then the surface of the workpiece treated in step 5 is electroplated with platinum.
[0055] In a preferred but non-limiting embodiment of the present invention, the method for electroplating platinum includes: using a [Pt(NH3)2(NO2)2] plating solution, the current density during electroplating is 0.4A / dm 2 ~5A / dm 2 The thickness of the platinum coating obtained is 2 to 10 microns.
[0056] like Figure 1 As shown, a thermal insulation coating according to the present invention comprises:
[0057] On the substrate surface from bottom to top are the bonding layer formed by the AlCr layer, the transition layer formed by the CrN / AlCrN layer, the intermediate layer formed by the CrON / AlCrON layer, the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer. The thermal insulation coating is also the Pt-Al2O3 / Cr2O3 / TiO2 composite coating.
[0058] In a preferred but non-limiting embodiment of the present invention, the thicknesses of the bonding layer formed by the AlCr layer, the transition layer formed by the CrN / AlCrN layer, the intermediate layer formed by the CrON / AlCrON layer, the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer are 1 to 10.0 microns, 1 to 10.0 microns, 1 to 10.0 microns, 5 to 60.0 microns and 3 to 10.0 microns, respectively.
[0059] In a preferred but non-limiting embodiment of the present invention, in the bonding layer formed by the AlCr layer, the Al content is 50-70 at.%; in the transition layer formed by the CrN / AlCrN layer, the Al content in the AlCrN layer is 50-70 at.%; in the intermediate layer formed by the CrON / AlCrON layer, the O content in the CrON layer is 10-20 at.%, and the N content is 20-30 at.%, the Al content in the AlCrON layer is 50-70 at.%, the O content is 10-20 at.%, and the N content is 20-30 at.%; in the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating, the Al content in the AlCrTi layer is 50-70 at.%; in the Al2O3 / Cr2O3 / TiO2 layer, the Al2O3 content is 50-70 at.%, the Cr2O3 content is 20-40 at.%, and the TiO2 content is 5-20 at.%.
[0060] The preparation method of the thermal insulation coating of the present invention is further described in detail below through examples.
[0061] Example 1
[0062] The substrate, that is, the workpiece, is made of 1Cr13Si2 heat-resistant steel, the sample size is 20mm×10mm×10mm, and the coating surface size is 20mm×10mm. The substrate surface is ground and sandblasted, ultrasonicated in an alcohol solution for 20 minutes, and then dried with hot air before being loaded on the workpiece rack in the vacuum chamber of the arc ion plating equipment; a high-purity aluminum-chromium target is used, and when the vacuum degree in the vacuum chamber reaches 5×10 -3Pa, start the workpiece holder rotation, adjust the speed to 2rpm, and heat the vacuum chamber to 450℃; introduce argon into the vacuum chamber, and control the gas pressure at 0.4Pa; adjust the substrate pulse negative bias to -220V, turn on the arc enhanced glow discharge ion source, make the gas glow discharge, and glow clean the sample for 55 minutes; adjust the argon flow rate to make the vacuum chamber pressure 0.8Pa, and turn on the aluminum chromium target arc source at the same time, with an arc current of 100A, adjust the pulse negative bias to -150V, adjust the pulse negative bias duty cycle to 60%, and deposit the transition layer formed by the AlCr layer for 20 minutes; then introduce nitrogen, and adjust the gas pressure to 3.0Pa , turn on the arc source of pure chromium target and aluminum-chromium alloy target, the arc current is 120A, adjust the pulse negative bias to -150V, adjust the pulse negative bias duty cycle to 60%, and deposit the transition layer formed by CrN / AlCrN layer for 15 minutes; then adjust the argon pressure to 0.3Pa, introduce nitrogen and oxygen, the nitrogen and oxygen flow ratio is 2:1, the vacuum chamber pressure is controlled at 0.9Pa, apply a pulse negative bias of -95V to the substrate, the pulse negative bias duty cycle is 50%, turn on the arc enhanced glow discharge ion source; adjust the arc current of chromium and aluminum-chromium alloy targets to 100A, and deposit CrON / AlCrON to form the intermediate layer for 10 minutes;
[0063] 3S1: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.3Pa, apply a pulsed negative bias voltage of -80V to the substrate, and the pulsed negative bias voltage duty cycle is 70%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 90A, and deposit the AlCrTi layer for 5 minutes;
[0064] 3S2: Use aluminum-chromium and aluminum-titanium alloy targets, introduce oxygen, adjust the vacuum chamber pressure to 0.9Pa, apply a pulsed negative bias voltage of -150V to the substrate, and the pulsed negative bias voltage duty cycle is 40%. Turn on the arc enhanced glow discharge ion source; adjust the aluminum-chromium and aluminum-titanium alloy target arc current to 90A, and deposit the Al2O3 / Cr2O3 / TiO2 layer for 5 minutes;
[0065] 3S3: Repeat steps 3S1 and 3S2 for a total of 20 times, and the total deposition time is controlled within 100 minutes;
[0066] 3S4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.4Pa, apply a pulsed negative bias voltage of -150V to the substrate, the pulsed negative bias voltage duty cycle is 50%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 90A, and the deposition time is 15 minutes;
[0067] After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source, stop the gas supply, continue to evacuate, continue to evacuate, cool with the furnace to below 100°C, open the vacuum chamber, and take out the workpiece.
[0068] The workpiece surface removed in the previous step is polished, and then the workpiece surface is electroplated with platinum using a [Pt(NH3)2(NO2)2] plating solution at a current density of 2.5A / dm 2 The thickness of the platinum coating obtained is 8 microns.
[0069] The total thickness of the obtained Pt-Al2O3 / Cr2O3 / TiO2 composite coating was 14.1 microns as tested by the ball scar method, and its thermal insulation effect was tested to be good.
[0070] Example 2
[0071] The substrate, that is, the workpiece, is made of 16Mn steel, the sample size is 20mm×10mm×10mm, and the coating surface size is 20mm×10mm. The substrate surface is ground and sandblasted, ultrasonicated in an alcohol solution for 20 minutes, and then dried with hot air before being loaded on the workpiece rack in the vacuum chamber of the arc ion plating equipment; a high-purity aluminum-chromium target is used, and when the vacuum degree in the vacuum chamber reaches 6×10 -3 Pa, start the workpiece holder rotation, adjust the speed to 3rpm, and heat the vacuum chamber to 420℃; introduce argon into the vacuum chamber, and control the gas pressure at 0.5Pa; adjust the substrate pulse negative bias to -200V, turn on the arc enhanced glow discharge ion source, make the gas glow discharge, and glow clean the sample for 45 minutes; adjust the argon flow rate to make the vacuum chamber pressure 0.6Pa, and turn on the aluminum chromium target arc source at the same time, with an arc current of 105A, adjust the pulse negative bias to -120V, adjust the pulse negative bias duty cycle to 55%, and deposit the transition layer formed by the AlCr layer for 18 minutes; then introduce nitrogen, and adjust the gas pressure to 2.0Pa , turn on the pure chromium target and the aluminum-chromium alloy target arc source, the arc current is 110A, adjust the pulse negative bias to -130V, adjust the pulse negative bias duty cycle to 50%, and deposit the transition layer formed by the CrN / AlCrN layer for 12 minutes; then adjust the argon pressure to 0.35Pa, introduce nitrogen and oxygen, the nitrogen and oxygen flow ratio is 2:1, the vacuum chamber pressure is controlled at 0.8Pa, apply a pulse negative bias of -85V to the substrate, the pulse negative bias duty cycle is 45%, and turn on the arc enhanced glow discharge ion source; adjust the chromium and aluminum-chromium alloy target arc current to 90A, and deposit CrON / AlCrON to form the German intermediate layer for 12 minutes;
[0072] 3S1: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.35Pa, apply a pulsed negative bias voltage of -90V to the substrate, and the pulsed negative bias voltage duty cycle is 50%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 90A, and deposit the AlCrTi layer for 6 minutes;
[0073] 3S2: Use aluminum-chromium and aluminum-titanium alloy targets, introduce oxygen, adjust the vacuum chamber pressure to 0.8Pa, apply a pulsed negative bias voltage of -130V to the substrate, and the pulsed negative bias voltage duty cycle is 45%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 95A, and deposit the Al2O3 / Cr2O3 / TiO2 layer for 6 minutes;
[0074] 3S3: Repeat steps 3S1 and 3S2 for 30 times, and the total deposition time is controlled at 180 min;
[0075] 3S4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.5Pa, apply a pulsed negative bias voltage of -110V to the substrate, the pulsed negative bias voltage duty cycle is 55%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 95A, and the deposition time is 12 minutes;
[0076] After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source, stop the gas supply, continue to evacuate, continue to evacuate, cool with the furnace to below 100°C, open the vacuum chamber, and take out the workpiece.
[0077] The workpiece surface removed in the previous step is polished, and then the workpiece surface is electroplated with platinum using a [Pt(NH3)2(NO2)2] plating solution at a current density of 3.5A / dm 2 The thickness of the platinum coating obtained is 6 microns.
[0078] The total thickness of the obtained Pt-Al2O3 / Cr2O3 / TiO2 composite coating was 17.8 microns as tested by the ball scar method, and its thermal insulation effect was tested to be good.
[0079] Example 3
[0080] The substrate, that is, the workpiece, is made of 1Cr13Si2 steel, the sample size is 20mm×10mm×10mm, and the coating surface size is 20mm×10mm. After grinding and sandblasting, the substrate surface is ultrasonically treated in an alcohol solution for 20 minutes, and then dried with hot air and loaded on the workpiece rack in the vacuum chamber of the arc ion plating equipment; a high-purity aluminum-chromium target is used. When the vacuum degree in the vacuum chamber reaches 5.5×10 -3Pa, start the workpiece holder rotation, adjust the speed to 4rpm, and heat the vacuum chamber to 480℃; introduce argon into the vacuum chamber, and control the gas pressure at 0.4Pa; adjust the substrate pulse negative bias to -180V, turn on the arc enhanced glow discharge ion source, make the gas glow discharge, and glow clean the sample for 40 minutes; adjust the argon flow rate to make the vacuum chamber pressure 0.4Pa, and turn on the aluminum chromium target arc source at the same time, with an arc current of 100A, adjust the pulse negative bias to -100V, adjust the pulse negative bias duty cycle to 50%, and deposit the transition layer formed by the AlCr layer for 16 minutes; then introduce nitrogen, and adjust the gas pressure to 2.2Pa , turn on the arc source of pure chromium target and aluminum-chromium alloy target, the arc current is 100A, adjust the pulse negative bias to -110V, adjust the pulse negative bias duty cycle to 55%, and deposit the transition layer formed by CrN / AlCrN layer for 14 minutes; then adjust the argon pressure to 0.45Pa, introduce nitrogen and oxygen, the nitrogen and oxygen flow ratio is 1:2, the vacuum chamber pressure is controlled at 0.6Pa, apply a pulse negative bias of -95V to the substrate, the pulse negative bias duty cycle is 40%, turn on the arc enhanced glow discharge ion source; adjust the arc current of chromium and aluminum-chromium alloy targets to 90A, and deposit CrON / AlCrON to form the intermediate layer for 10 minutes;
[0081] 3S1: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.55Pa, apply a pulsed negative bias voltage of -95V to the substrate, and the pulsed negative bias voltage duty cycle is 60%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 95A, and deposit the AlCrTi layer for 5 minutes;
[0082] 3S2: Use aluminum-chromium and aluminum-titanium alloy targets, introduce oxygen, adjust the vacuum chamber pressure to 0.5Pa, apply a pulsed negative bias voltage of -150V to the substrate, and the pulsed negative bias voltage duty cycle is 40%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 105A, and deposit the Al2O3 / Cr2O3 / TiO2 layer for 5 minutes;
[0083] 3S3: Repeat steps 3S1 and 3S2 for 30 times, and the total deposition time is controlled at 150 minutes;
[0084] 4S4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.2Pa, apply a pulsed negative bias voltage of -140V to the substrate, the pulsed negative bias voltage duty cycle is 45%, turn on the arc enhanced glow discharge ion source; adjust the aluminum-chromium and aluminum-titanium alloy target arc current to 85A, and the deposition time is 10 minutes;
[0085] After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source, stop the gas supply, continue to evacuate, continue to evacuate, cool with the furnace to below 100°C, open the vacuum chamber, and take out the workpiece.
[0086] The workpiece surface removed in the previous step is polished, and then the workpiece surface is electroplated with platinum using a [Pt(NH3)2(NO2)2] plating solution at a current density of 3.2A / dm 2 The thickness of the platinum coating obtained is 7 microns.
[0087] The total thickness of the obtained Pt-Al2O3 / Cr2O3 / TiO2 composite coating was 17.2 microns as tested by the ball scar method, and its thermal insulation effect was tested to be good.
[0088] Example 4
[0089] The substrate, that is, the workpiece, is made of GH4169 high-temperature alloy. The sample size is 20mm×10mm×10mm, and the coating surface size is 20mm×10mm. The substrate surface is ground and sandblasted, ultrasonicated in an alcohol solution for 20 minutes, and then dried with hot air before being loaded on the workpiece rack in the vacuum chamber of the arc ion plating equipment; a high-purity aluminum-chromium target is used. When the vacuum degree in the vacuum chamber reaches 4×10 -3 Pa, start the workpiece holder rotation, adjust the speed to 3rpm, and heat the vacuum chamber to 430℃; introduce argon into the vacuum chamber, and control the gas pressure at 0.8Pa; adjust the substrate pulse negative bias to -200V, turn on the arc enhanced glow discharge ion source, make the gas glow discharge, and glow clean the sample for 40 minutes; adjust the argon flow rate to make the vacuum chamber pressure 0.7Pa, and turn on the aluminum chromium target arc source at the same time, with an arc current of 95A, adjust the pulse negative bias to -110V, adjust the pulse negative bias duty cycle to 45%, and deposit the transition layer formed by the AlCr layer for 16 minutes; then introduce nitrogen, and adjust the pressure to 1.8Pa , turn on the pure chromium target and the aluminum-chromium alloy target arc source, the arc current is 105A, adjust the pulse negative bias to -110V, adjust the pulse negative bias duty cycle to 50%, and deposit the transition layer formed by the CrN / AlCrN layer for 10 minutes; then adjust the argon pressure to 0.4Pa, introduce nitrogen and oxygen, the nitrogen and oxygen flow ratio is 1:1, the vacuum chamber pressure is controlled at 0.6Pa, apply a pulse negative bias of -105V to the substrate, the pulse negative bias duty cycle is 43%, and turn on the arc enhanced glow discharge ion source; adjust the chromium and aluminum-chromium alloy target arc current to 80A, and deposit the intermediate layer formed by CrON / AlCrON for 10 minutes;
[0090] 3S1: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.45Pa, apply a pulsed negative bias voltage of -95V to the substrate, and the pulsed negative bias voltage duty cycle is 55%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 95A, and deposit the AlCrTi layer for 8 minutes;
[0091] 3S2: Use aluminum-chromium and aluminum-titanium alloy targets, introduce oxygen, adjust the vacuum chamber pressure to 0.8Pa, apply a pulsed negative bias voltage of -100V to the substrate, and the pulsed negative bias voltage duty cycle is 40%. Turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 90A, and deposit the Al2O3 / Cr2O3 / TiO2 layer for 8 minutes;
[0092] 3S3: Repeat steps 3S1 and 3S2 for 16 times, and the total deposition time is controlled at 128 minutes;
[0093] 4S4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure to 0.6Pa, apply a pulsed negative bias voltage of -140V to the substrate, the pulsed negative bias voltage duty cycle is 40%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 95A, and the deposition time is 15 minutes;
[0094] After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source, stop the gas supply, continue to evacuate, continue to evacuate, cool with the furnace to below 100°C, open the vacuum chamber, and take out the workpiece.
[0095] The workpiece surface removed in the previous step is polished, and then the workpiece surface is electroplated with platinum using a [Pt(NH3)2(NO2)2] plating solution at a current density of 1.5A / dm 2 The thickness of the platinum coating obtained is 4 microns.
[0096] The total thickness of the obtained Pt-Al2O3 / Cr2O3 / TiO2 composite coating was 12.7 microns as tested by the ball scar method, and its thermal insulation effect was tested to be good.
[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a thermal insulation coating, characterized in that: include: Step 1: Pre-cleaning of workpiece; Step 2: Plating a transition layer on the pre-cleaned workpiece; Step 3: Plating a CrON / AlCrON intermediate layer on the workpiece after the transition layer is plated; Step 4: Plating the workpiece after plating the CrON / AlCrON intermediate layer with an AlCrTi / Al2O3 / Cr2O3 / TiO2 layer; Step 5: After the deposition is completed, turn off the arc power supply, pulse negative bias voltage, and ion source in the vacuum chamber, stop the gas supply, continue to evacuate the vacuum chamber, cool it to below 100°C with the furnace, open the vacuum chamber, and take out the workpiece processed in step 5; Step 6: Plate a Pt layer on the workpiece processed in step 5.
2. The method for preparing the thermal insulation coating according to claim 1, characterized in that: Step 1 specifically includes: after the workpiece surface is ground and sandblasted, it is ultrasonicated in an alcohol solution for 10 to 20 minutes, and then dried with hot air and loaded on a workpiece rack in a vacuum chamber to wait for coating.
3. The method for preparing the thermal insulation coating according to claim 2, characterized in that: Step 2 specifically includes: using a high-purity aluminum-chromium target arc source in a vacuum chamber, when the vacuum degree in the vacuum chamber reaches 1×10 -3 Pa~1×10 -2 When the temperature reaches 0.0400°C, the workpiece holder is turned on and the rotation speed is adjusted to 1-4 rpm, and the vacuum chamber is heated to 300-500°C; argon gas is introduced into the vacuum chamber, and the gas pressure is controlled between 0.3 and 6 Pa; the pre-cleaned workpiece, that is, the substrate, is subjected to a pulsed negative bias voltage in the range of -50 to -600 V, and the arc enhanced glow discharge ion source is turned on and the gas is glow discharged, and the pre-cleaned workpiece, that is, the sample, is glow cleaned for 20 to 60 minutes; the argon gas flow rate is adjusted so that the vacuum chamber pressure is 0.02 to 1.0 Pa, and the high-purity aluminum chromium The target arc source has an arc current of 50 to 200A, the pulse negative bias is adjusted to -50V to -500V, the duty cycle of the pulse negative bias is adjusted to 20% to 80%, and the transition layer formed by the AlCr layer is deposited for 5 to 40 minutes; then nitrogen is introduced into the vacuum chamber, the gas pressure is adjusted to 0.5 to 5.0Pa, the pure chromium target and the high-purity aluminum-chromium alloy target arc source are turned on, the arc current is 50 to 200A, the pulse negative bias is adjusted to -50V to -500V, the duty cycle of the pulse negative bias is adjusted to 20% to 80%, and the transition layer formed by the CrN / AlCrN layer is deposited for 4 to 40 minutes.
4. The method for preparing the thermal insulation coating according to claim 3, characterized in that: Step 3 specifically includes: using a chromium target and an aluminum-chromium alloy target, adjusting the argon pressure in the vacuum chamber to 0.1-0.5 Pa, introducing nitrogen and oxygen, with the nitrogen and oxygen flow ratio in the range of 2:1-1:2, and controlling the pressure at 0.2-1.5 Pa, applying a pulsed negative bias voltage of -50V to -300V to the workpiece after the transition layer is plated, that is, substrate 2, with a pulsed negative bias voltage duty cycle of 20% to 80%, and turning on the arc enhanced glow discharge ion source; adjusting the arc current of the chromium target and the aluminum-chromium alloy target to 50-200A, and the deposition time to 5-20 minutes.
5. The method for preparing the thermal insulation coating according to claim 4, characterized in that: Step 4 specifically includes: Step 4-1: Using aluminum-chromium and aluminum-titanium alloy targets, adjusting the argon gas pressure in the vacuum chamber to 0.1-2 Pa, applying a pulsed negative bias voltage of -50V to -300V to the workpiece after the CrON / AlCrON intermediate layer is plated, that is, the substrate three, and the pulsed negative bias voltage duty cycle is 20% to 80%, turning on the arc enhanced glow discharge ion source; adjusting the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50-200A, and the deposition time to 1 to 10 minutes; Step 4-2: Then, oxygen is introduced into the vacuum chamber, and the vacuum chamber pressure is adjusted to 0.2-2.0 Pa. A pulsed negative bias voltage of -50V--300V is applied to the substrate three, and the pulsed negative bias voltage duty ratio is 20%-80%, and the arc enhanced glow discharge ion source is turned on; the target arc current of aluminum-chromium and aluminum-titanium alloy is adjusted to 50-200A, and the deposition time is 1-10 minutes; Step 4-3: Repeat steps 4-1 to 4-2 for 10 to 50 times, and the total deposition time is controlled within 30 to 300 minutes; Step 4-4: Use aluminum-chromium and aluminum-titanium alloy targets, adjust the argon gas pressure in the vacuum chamber to 0.1~2Pa, apply a pulsed negative bias voltage of -50V~-300V to the substrate three, and the pulsed negative bias duty cycle is 20%~80%, turn on the arc enhanced glow discharge ion source; adjust the arc current of the aluminum-chromium and aluminum-titanium alloy targets to 50~200A, and the deposition time is 10~30 minutes.
6. The method for preparing the thermal insulation coating according to claim 5, characterized in that: Step 6 specifically includes: The surface of the workpiece taken out after being processed in step 5 is polished, and then the surface of the workpiece treated in step 5 is electroplated with platinum.
7. The method for preparing the thermal insulation coating according to claim 6, characterized in that: The method for electroplating platinum includes: using [Pt(NH3)2(NO2)2] plating solution, the current density during electroplating is 0.4A / dm 2 ~5A / dm 2 The thickness of the platinum coating obtained is 2 to 10 microns.
8. A thermal insulation coating, characterized in that: include: On the substrate surface from bottom to top are the bonding layer formed by the AlCr layer, the transition layer formed by the CrN / AlCrN layer, the intermediate layer formed by the CrON / AlCrON layer, the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer. The thermal insulation coating is also the Pt-Al2O3 / Cr2O3 / TiO2 composite coating.
9. The thermal insulation coating according to claim 8, characterized in that: The bonding layer is formed by the AlCr layer, the transition layer is formed by the CrN / AlCrN layer, and the intermediate layer is formed by the CrON / AlCrON layer. The thicknesses of the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating and the Pt surface layer are 1-10.0 microns, 1-10.0 microns, 1-10.0 microns, 5-60.0 microns and 3-10.0 microns, respectively.
10. The thermal insulation coating according to claim 9, characterized in that: In the bonding layer formed by the AlCr layer, the Al content is 50-70at.%; in the transition layer formed by the CrN / AlCrN layer, the Al content in the AlCrN layer is 50-70at.%; in the intermediate layer formed by the CrON / AlCrON layer, the O content in the CrON layer is 10-20at.%, and the N content is 20-30at.%, and the Al content in the AlCrON layer is 50-70at.%, the O content is 10-20at.%, and the N content is 20-30at.%; in the AlCrTi / Al2O3 / Cr2O3 / TiO2 composite coating, the Al content in the AlCrTi layer is 50-70at.%; in the Al2O3 / Cr2O3 / TiO2 layer, the Al2O3 content is 50-70at.%, the Cr2O3 content is 20-40at.%, and the TiO2 content is 5-20at.%.
Citation Information
Patent Citations
A method for welding workpieces made of high-temperature superalloys with a special quality delivery rate of welding additives.
CN102639283B